1. What Requirements Does the Iron and Steel Smelting Process Place on Refractories?
In the iron and steel smelting process, refractories should meet the following requirements:
① A relatively wide service temperature range, generally up to 1760 °C;
② The ability to withstand rapid temperature fluctuations, i.e. good thermal shock resistance, so as to prevent the lining refractories from cracking and fracturing;
③ The ability to withstand moderate compressive stress at both high and low temperatures;
④ The ability to withstand friction (abrasion) at both high and low temperatures;
⑤ Resistance to slag attack, both acidic and basic slag;
⑥ The ability to withstand the enormous hydrostatic pressure and buoyancy of molten metal;
⑦ The ability to withstand the action of furnace gases - including CO, SO₂, CO₂, CH₄, H₂O, and the volatile oxides and salts contained in the metal - and to prevent them from penetrating into the refractories and reacting with them.
Because refractories have to withstand the conditions described above, they normally serve as an efficient isolating (barrier) layer; in some cases they are also required to act as a heat conductor or a heat absorber, depending on the specific application.
2. What Are Magnesia–Carbon Bricks?




Magnesia–carbon bricks are a product that has evolved in recent years from tar-bonded bricks and burned oil-impregnated bricks. They are made from sintered magnesite or fused magnesia and carbon material (graphite) as raw materials, with carbon-containing resin as the binder, through mixing, pressing, and heat treatment at about 220 °C, in which the carbon forms a continuous network phase that envelops the periclase grains. The main characteristics of magnesia–carbon bricks are as follows.
① During press-forming, graphite tends to assume a lamellar structure, and the bonding between graphite particles and between graphite and periclase is poor, leaving the body rather loose. The cold strength of magnesia–carbon bricks is therefore low, and high-pressure pressing is essential if density and strength are to be increased.
② Graphite has low thermal expansion and high thermal conductivity, which gives magnesia–carbon bricks good thermal shock resistance.
③ Graphite is not wetted by slag and has very high chemical stability; consequently, when the carbon in a magnesia–carbon brick forms a continuous network, the brick possesses strong slag resistance.
④ The carbon in magnesia–carbon bricks is highly susceptible to oxidation. Baking at low temperature must therefore be carried out under air-excluded conditions, and the bricks cannot be fired in air. Adding small amounts of fine powders of Al, Si, Mg and carbides can also prevent oxidation of the carbon.
3. What Are the Characteristics of Bricks Used in BOF Linings?
At present, magnesia–carbon bricks are the material generally used for BOF (basic oxygen furnace) linings. They have strong slag resistance and good thermal conductivity, which prevents the thermal cracking of magnesia grains; at the same time, the carbon network formed after the binder has cured binds the magnesia (MgO) grains tightly and firmly together.
A BOF lining consists of an insulating layer, a permanent (safety) layer and a working layer. The insulating layer is generally built of polycrystalline refractory fibre; at the furnace hood, the insulating layer is sometimes rammed from resin-bonded magnesia. The bricks used for the permanent layer differ from one zone to another: it is mostly built of low-grade magnesia–carbon bricks, tar-bonded dolomite bricks or sintered magnesia bricks. The working layer is built entirely of magnesia–carbon bricks.
4. How Is a BOF Lining Built with Combined (Zoned) Bricklaying?
The working layer of a BOF is in direct contact with high-temperature molten steel and slag. It is chemically attacked by high-temperature slag, scoured by molten steel, slag and furnace gases, and subjected to mechanical impact during scrap charging, so its service conditions are very severe. During blowing, because the working conditions differ from zone to zone, the pattern and amount of lining wear also differ. In view of this, refractories of different materials, or of the same material in different grades, are laid according to the severity of damage at each location - this is what is known as combined lining (zoned bricklaying) of the furnace.
(1) Furnace mouth. Magnesia–carbon bricks are used here that have high thermal shock resistance and slag resistance, withstand the scouring of molten slag and hot waste gas, and do not readily stick to steel - and if steel does stick, it is easy to clean off.
(2) Furnace cone (hood section). This is the zone most severely attacked by slag; it is also affected by rapid temperature changes and scoured by dust-laden waste gas, so magnesia–carbon bricks with strong slag resistance and good thermal shock resistance are used.
(3) Charging side of the lining. Magnesia–carbon bricks with high slag resistance, high strength, high thermal shock resistance and added antioxidants are laid here.
(4) Tapping side of the lining. This side is less affected by thermal shock but more strongly affected by the thermal impact and scouring of molten steel. Magnesia–carbon bricks of the same grade as on the charging side are normally used, but may be somewhat thinner.
(5) Trunnion areas on both sides. Besides wear during blowing, these areas are not covered by slag, so the carbon in the bricks oxidizes very readily; magnesia–carbon bricks with strong oxidation resistance should be laid here.
(6) Slag line. This zone suffers relatively severe slag attack and requires magnesia–carbon bricks with good slag resistance; grade MT14A magnesia–carbon bricks may also be selected.
(7) Bath and furnace bottom. These areas are eroded by molten steel, but the damage is lighter than elsewhere; grade MT14B magnesia–carbon bricks with a lower carbon content may be used.
5. What Are the Characteristics of the Bricks Used at the Taphole and at the Furnace Bottom?
The taphole is subjected to erosion by high-temperature molten steel and to sharp temperature changes, so it is damaged rather severely. It should therefore be built of one-piece magnesia–carbon bricks or composite (assembled) magnesia–carbon bricks with high erosion resistance and oxidation resistance; one-piece bricks or composite bricks (e.g. MT14A) are generally used, and they must be replaced after 200 heats.
Bottom-blowing bricks are used to inject Ar, N₂ or CO₂, or mixtures of these with oxygen, through the furnace bottom. Combined blowing generates high temperatures and vigorous stirring, so the bottom-blowing bricks must be resistant to high temperature, erosion, scouring, abrasion and spalling; from the standpoint of blowing, the gas passing through the bricks must produce fine, uniform bubbles; and the bricks must be safe and reliable in service, with a service life matched as far as possible to that of the lining. For these reasons, magnesia–carbon material remains the best choice.
6. What Process Properties Should Refractories for Throw-in Patching of BOF Linings Have?
The patching material is thrown into the furnace through the mouth and the vessel is rocked; under the residual heat in the furnace, the material becomes fluid and spreads over the worn areas of the lining.
The patching material should have the following process properties:
① Good spreadability at the residual-heat temperature of the BOF lining (800–1200 °C).
② Rapid solidification after spreading.
③ Good adhesion to the original lining material after solidification.
④ Good erosion resistance of the patched material itself.
The patching material is based on magnesia or magnesia–dolomite sand, and its process properties depend mainly on the binder. The binders commonly used are pitch, resin, or a mixture of the two. Because of its low price and ease of use, the patching material actually used in Chinese steel plants is pitch-bonded.
7. What Gunning Methods Are Used for BOF Linings, and What Are the Characteristics of the Refractories Involved?
Where the lining is locally damaged (for example at the trunnion areas) but patching material is unsuitable, gunning technology can be used: refractory is sprayed intensively onto the severely worn areas so that it sinters into one body with the lining bricks, thus repairing the lining. Gunning methods include dry gunning, semi-dry gunning and flame gunning; at present semi-dry gunning is mostly used.
The gunning mix may be magnesia or high-magnesia dolomite, with a particle size below 0.1 mm, of which more than 60% is finer than 0.09 mm. Pulverized coal or aluminium powder, etc., may be used as fuel. Plasticizing and sintering agents include soft clay, bentonite or wollastonite. Some plants also blend lime and other slag-forming agents into the gunning mix so that the flame-gunned layer becomes a refractory slag layer protecting the original brick layer of the lining, and this has given good results in practice.
In China, metallurgical magnesia is mostly used for gunning mixes. The binders commonly used are solid water glass, i.e. sodium silicate (Na₂O·nSiO₂), chromates, phosphates (sodium tripolyphosphate), etc.; in addition, a suitable amount of carboxymethyl cellulose may be added. The quantity of gunning mix used depends on the extent of damage; after gunning, whether drying is required and for how long depends on the amount of mix applied. The compositions of wet and semi-dry gunning mixes are given in Table 3.
| Gunning method | MgO (wt%) | CaO (wt%) | SiO₂ (wt%) | >1.0 mm (%) | <1.0 mm (%) | Moisture (%) |
|---|---|---|---|---|---|---|
| Wet | 91 | 1 | 3 | 10 | 90 | 15–17 |
| Semi-dry | 90 | 5 | 2.5 | 25 | 75 | 10–17 |
Table 3 Composition of the Gunning Mix
8. What Is Slag Splashing for BOF Lining Protection, and What Are the Requirements on End-Point Slag Composition?
Slag splashing is the principal means of maintaining a BOF lining. Its basic principle is as follows: after the steel has been fully tapped at the end of blowing, part of the end-point slag, whose MgO content is saturated or supersaturated, is left in the furnace; high-pressure nitrogen (0.8–0.9 MPa) is blown through a lance positioned 0.8–2.0 m above the theoretical bath level, and the high-velocity nitrogen jet splashes the slag up so that it forms a high-melting-point slag coating on the lining surface and bonds well to the lining, thereby protecting the lining and extending the campaign life.
Slag splashing places no special requirement on the w(TFe) of the end-point slag: as long as the w(MgO) in the slag is adjusted to a suitable range before splashing, the desired slag-splashing effect can be achieved.
There are two ways of adjusting the slag composition. One is to add the slag conditioner together with the slag-forming materials when blowing starts, so that the end-point slag composition - in particular w(MgO) - reaches the target, and no further conditioner is needed after tapping. If the end-point slag composition fails to meet the requirements for slag splashing, the other way is used: a slag conditioner is added after tapping to bring the w(MgO) into the range required for slag splashing.
9. What Types of Slag Conditioners Are Used in Slag Splashing, and What Are Their Characteristics?
The slag conditioners commonly used are lightly calcined dolomite, raw dolomite, lightly calcined magnesia pellets, metallurgical magnesia, magnesite slag and high-magnesia lime. The main function of a slag conditioner is to raise the MgO content of the slag. In selecting a conditioner, its MgO content is the first consideration. Taking all factors into account, the concept of the "MgO mass fraction" has been introduced to compare the MgO levels of different conditioners. The MgO mass fraction is defined as follows:
![]()
w(MgO),w(CaO),w(SiO₂) are the actual MgO, CaO and SiO₂ contents of the slag conditioner; B is the slag basicity, which may be taken as B = 3.5.
The compositions of the commonly used slag conditioners are given in Table 4. When selecting a conditioner on the basis of MgO content, metallurgical magnesia, lightly calcined magnesia pellets, lightly calcined dolomite and magnesia-bearing lime are to be preferred (MgO mass fraction not less than 50%). Obviously, from the cost point of view, the cheaper conditioner should be chosen.
| Type | w(CaO) | w(SiO₂) | w(MgO) | Loss on ignition | MgO mass fraction |
|---|---|---|---|---|---|
| Raw dolomite | 30.3 | 1.95 | 21.7 | 44.48 | 28.4 |
| Lightly calcined dolomite | 51.0 | 5.5 | 37.9 | 5.6 | 55.5 |
| Magnesite slag granules | 0.8 | 1.2 | 45.9 | 50.7 | 44.4 |
| Lightly calcined magnesia pellets | 1.5 | 5.8 | 67.4 | 22.5 | 56.7 |
| Metallurgical magnesia | 8 | 5 | 83 | 0.8 | 75.8 |
| High-magnesia lime | 81 | 3.2 | 15 | 0.8 | 49.7 |
Table 4 Compositions of Common Slag Conditioners (unit: %)
From the comparison of the above materials, raw dolomite has the lowest cost; lightly calcined dolomite and magnesite slag granules are moderately priced; high-magnesia lime, metallurgical magnesia and lightly calcined magnesia pellets are relatively expensive.