Ladle Vent Bricks
Tangshan Iron and Steel's No. 1 Rolling Mill uses integral vent bricks in its refining ladles. During operation, issues such as spalling, steel entrapment in crevices, and failure to open fully have been observed. Measurements indicate that the residual brick core length is approximately 180mm, with a monthly permeability rate of 99.2%. By analyzing the causes of vent brick damage and implementing corresponding measures, the core length of the vent bricks can be increased, which will improve the permeability rate.
01 Analysis of Causes for Vent Brick Damage
1.1 Delamination of Vent Brick Core
Following hot repairs of the ladle, when positioning the ladle for the converter, the internal temperature is approximately 900°C, while the final temperature of the converter is typically around 1630°C. The extreme thermal shock caused by this temperature differential leads to delamination of the vent brick core, with the delaminated layer typically measuring 10–20mm in thickness. Furthermore, once delaminated, the tapered section of the core does not detach, impairing the permeability of the molten steel within the ladle.
1.2 Fracture of Vent Brick Base Bricks
The thermal shock induced by temperature differentials can also cause fractures in the base bricks of the vent brick, with fracture heights ranging from 100 to 200mm. Without the protection of the base bricks, the core becomes susceptible to erosion by molten steel and may fracture. Such fractures pose significant hazards, particularly during the later stages of vent brick usage when the residual brick height is reduced, increasing the risk of molten steel leakage from the ladle bottom.
1.3 Low Strength and Poor Erosion Resistance
During hot repairs, an oxygen lance is used to clear the vent bricks, with the standard clearance rate being 9–12mm per furnace. If the strength of the vent brick core is insufficient, the core height visibly diminishes with each clearance. As a result, the vent bricks fail prematurely, before reaching their specified service life, disrupting ladle rotation and causing production instability.
1.4 Erosion Damage from Molten Steel Scouring
During inert gas injection through the vent brick, gas flow recoil exerts impact forces on the exposed periphery. The interaction between high-velocity molten steel and gas currents generates swirling eddies. When the vent brick protrudes above the vent seat, its exposed section undergoes scouring and shearing by these eddies, forming annular grooves.
1.5 Damage from Excessive Oxygen Burning
When the ladle's return pouring is delayed after continuous casting completion, cold steel accumulates at the ladle bottom. This necessitates oxygen lance cleaning by directing the flame against the vent brick core. Such direct burning causes rapid damage to the core.
1.6 Vent Brick Core Burning Off-Center
When cleaning the vent brick by pressing the oxygen lance against its core, the concentrated oxygen flow at a single point can cause the core to burn unevenly. This results in a non-planar surface with a height difference exceeding 50mm. Uneven burning impairs the brick's permeability, and each subsequent cleaning exacerbates the deviation, leading to premature decommissioning.
1.7 Low Back-Blow Gas Pressure
The back-blow gas is nitrogen at a pressure of 0.5 MPa, while the oxygen lance operates at 0.8 MPa. During oxygen-fired cleaning, molten steel can be blown into the vent brick's narrow gaps. Upon cooling, this solidifies and blocks the gaps, impairing venting. Subsequent hot repairs and cleanings further exacerbate the burn damage to the vent brick core.
1.8 Erosion of Corundum Material and Base Bricks around Vent Bricks
During base bricklaying, corundum self-flowing material is poured around the vent brick seat with a width of 50–100mm to protect the seat bricks. Due to insufficient strength of the corundum self-flowing material or construction issues, the corundum material around the vent brick seat may detach. Molten steel infiltration can then cause the fracture of the vent seat brick. Alternatively, the fracture of the hearth bricks surrounding the vent seat brick may occur, which, in turn, causes the fracture of the surrounding corundum material and the vent seat brick.
02 Measures to Enhance the Quality of Ventilating Bricks
2.1 Incorporating Zirconium-Based Materials and Plate-Shaped Corundum to Improve the Flaking Resistance of Ventilating Bricks
Incorporating pre-synthesized zirconium-based materials into ventilating bricks modifies the properties of aluminum-chromium bricks. By leveraging the toughening effect of ZrO₂, the thermal shock stability of the bricks can be significantly enhanced. Plate-shaped corundum, which has high strength, endows the bricks with excellent thermal volume stability and good thermal shock resistance.
2.2 Enhancing the Erosion Resistance and Strength of Vent Bricks
Minimize impurity content in raw materials to improve the high-temperature performance of vent bricks. Adding α-Al₂O₃ micropowder and spinel with particle sizes ranging from 1–0 mm, at a controlled dosage of 16%–20%, increases the strength of the vent bricks, thereby enhancing their resistance to oxygen purging.
03 Standardizing On-Site Operations
3.1 Promptly Returning Residual Steel
If residual steel is not promptly returned after completing continuous casting, cold steel will form at the ladle bottom, and slag crusts will develop. This complicates vent brick cleaning, compromises permeability, and prolonged oxygen-fired cleaning accelerates vent brick deterioration. Therefore, the time between the completion of continuous casting and the return of residual steel must be regulated. Field data indicates that residual steel remains fluid for up to 10 minutes, though this depends on refining exit temperature, steel grade, and ladle condition.
3.2 Strictly Prohibiting Oxygen Burner Operation Against Vent Bricks
When cleaning vent bricks with the oxygen lance, the lance tip must not be pressed against the brick core during operation. This accelerates brick deterioration and increases the risk of uneven burning. Maintain a distance of approximately 50mm between the lance tip and the brick core.
3.3 Installation of Flow Meters
A contributing factor to excessive oxygen burning during vent brick cleaning is reliance on operator experience. A blackened vent brick core accompanied by gas-related noise is often interpreted as evidence of good venting. To prevent excessive burn-through and eliminate reliance on subjective experience, flow meters should be installed at the ladle hot repair station. Set an alarm threshold corresponding to the venting capacity required for argon blowing during refining, using both audible and visual alarms. Operators should cease operation upon reaching the flow alarm, thereby reducing human-induced damage to the venting bricks and eliminating judgmental bias regarding their venting performance.
3.4 Enhancing Backflush Gas Pressure
The backflush gas was upgraded from low-pressure nitrogen to high-pressure nitrogen, increasing the pressure from 0.5 MPa to 1.2 MPa. This upgrade prevents molten steel from entering the gaps. Concurrently, the backblowing duration was adjusted: instead of starting backblowing when the ladle is placed on the ladle turner, it now begins only after the nozzle has been cleaned and before vent brick cleaning. This shortens the backblowing time, preventing excessive core temperature drop during prolonged backblowing, which could lead to delamination.
3.5 Slag Control
Prior to adding flow sand during ladle hot repair, the ladle is tilted approximately 45° downward using the tilting mechanism to perform slag control operations. This prevents thin slag from flowing back and blocking the vent bricks when the ladle is upright, thereby maintaining adequate permeability and ensuring production continuity.
3.6 Ladle Bottom Lining
First, use pneumatic hammers to remove loose ladle bottom bricks. If embedded steel is encountered between layers or cracks appear in the bricks, remove refractories until all hazards are eliminated. If permanent layers around seat bricks detach due to mechanical vibration or damage during removal, all unsupported bottom bricks must be dismantled until intact sintered permanent layers are exposed. Finally, measure the residual brick thickness. The remaining thickness of the lining bricks around the permeable bricks and water seat bricks must not be less than 200mm. Any lining bricks with a thickness below 200mm must be completely removed using an air hammer.
3.7 Corundum Material Application
Using a mixer and materials, the weight ratio of corundum material to water should be 1:0.05–0.08 (1:0.05–0.07 in winter). Water must be measured using a dedicated measuring bucket. Wet mixing time should be 5–10 minutes, using clean water only-no wastewater. The mixed material should exhibit no separation of water and aggregate, maintaining fluidity. Pour the free-flowing corundum mixture into the gap between the base-enveloping air vent bricks and the base-enveloping bricks. Apply a vibrator around the perimeter of the air vent bricks for two full rotations, vibrating for 1.5 to 2 minutes.
Through enhanced air vent brick quality and further standardization of on-site operations, the erosion rate of air vent bricks has significantly decreased, with both service life and residual brick length improved. See Table 1 for details.

04 Conclusion
Through the implementation of various measures, the permeability rate of the ladle has increased to 99.9%, ensuring both the quality of the molten steel and the stability of production. At the same time, the residual brick core length has reached 196mm, laying the groundwork for extending the service life of the permeable bricks and enhancing the ladle's life in subsequent stages.