Application And Damage Mechanism Of Magnesia-Carbon Bricks in Ladles

May 26, 2026

Leave a message

 

Application and Damage Mechanism of Magnesia-Carbon Bricks in Ladles

 

 

Magnesia-Carbon Bricks for Steel Ladles

 

In steel ladles, the chemical composition of slag is complex and variable, accompanied by drastic and frequent temperature fluctuations. For this reason, high-performance magnesia-carbon bricks are generally adopted at the slag line of steel ladles. Extensive research has been conducted domestically and internationally on the erosion mechanism of magnesia-carbon bricks used in steel ladles. A detailed summary is presented as follows.

 

Erosion of Magnesia-Carbon Bricks by Slag

 

The slag line of steel ladles suffers the most severe lining damage due to its complex physicochemical environment. The chemical erosion of magnesia-carbon bricks by steel slag mainly results from the dissolution of magnesia and the oxidation of graphite inside the bricks. The combined effect of these two factors leads to the deterioration of magnesia-carbon bricks.

 

Effect of Slag Basicity

 

Lower slag basicity aggravates the erosion of magnesia-carbon bricks. As slag basicity rises, the activity of FeO in slag decreases, which further weakens the diffusion capacity of FeO and thereby mitigates slag erosion on the bricks.

 

Effect of MgO

 

The reaction layer of residual bricks at the slag line of LF ladles contains a high content of MgO. When the MgO content in slag is low, the erosion rate of magnesia-carbon bricks rises sharply. Moreover, lower slag basicity will further accelerate the erosion process.

 

Effect of Al₂O₃

 

Alumina in slag reduces the melting point and viscosity of slag, which significantly enhances the penetration and erosion of slag against magnesia-carbon bricks. In addition, Al₂O₃ erodes magnesia along grain boundaries and causes the dissociation of periclase.

 

Effect of FeO

 

Firstly, FeO in slag readily reacts with graphite in magnesia-carbon bricks via oxidation at high temperatures, forming bright white iron beads and decarburized layers. Secondly, magnesia reacts with FeO in slag to form low-melting-point magnesiowüstite. During repeated heating and cooling cycles of the steel ladle, phase transformation between magnesiowüstite and magnesioferrite is accompanied by volume changes, which generates cracks on the working surface of periclase and accelerates its dissolution.

 

Overseas studies indicate that a higher iron content in steel slag shortens the service life of magnesia-carbon bricks. On one hand, iron oxides accelerate graphite oxidation; on the other hand, they increase the solubility of MgO in slag and speed up the dissolution of periclase. The synergistic action of the above two factors eventually causes the erosion of magnesia-carbon bricks.

 

Oxidation of Carbon in MgO-C Bricks

 

Oxidation of carbon on the hot face of the working lining gives rise to a thin decarburized layer, which is the primary cause for the damage of magnesia-carbon bricks. Carbon is continuously oxidized under the action of carbon dioxide, oxygen, silica and other oxides in the atmosphere, as well as iron oxides in slag. Meanwhile, it is also affected by the vaporization of magnesia inside the bricks and molten steel.

 

Furthermore, high-temperature molten slag continuously penetrates into pores and thermally induced cracks within the decarburized layer, and reacts with magnesia to form new low-melting compounds. Subjected to intense mechanical stirring and slag scouring, the surface layer of the bricks deteriorates and weakens, and eventually peels off layer by layer, resulting in severe damage to the magnesia-carbon bricks.

 

When the temperature exceeds a certain threshold, the brick structure is destroyed and its erosion accelerates sharply. This phenomenon occurs because magnesia starts to react with graphite at elevated temperatures.

 

Effect of Pores

 

The presence of open pores in magnesia-carbon bricks accelerates their degradation. During service, pores act as a catalyst for carbon oxidation, which further intensifies slag erosion on the brick lining.

 

Ambient air penetrates into the open pores and cools the brick. Oxygen in the air reacts with the surrounding carbon to produce carbon monoxide, which then exits through the pores as the temperature rises. The continuous repetition of this cycle gradually increases the porosity.

 

Binder is a major factor contributing to pore formation in magnesia-carbon bricks, and phenolic resin is the main component of common binders. A low dosage of phenolic resin results in a final porosity of approximately 3%. However, phenolic resin decomposes upon heating and generates gases including water vapor, hydrogen, methane, carbon monoxide and carbon dioxide. The flow of these gases creates pores and raises the overall porosity.

 

Consequently, the bricks are continuously attacked by oxides in the infiltrating slag and oxygen from the air. Both carbon oxidation and the reaction between slag and magnesia in the bricks become more vigorous, leading to brick damage. This cyclic process keeps worsening the deterioration of magnesia-carbon bricks.