Analysis of the Causes of Damage to Magnesium Carbon Bricks in Ladles and the Influence of Erosion Rates
Establishing a safety utilization system centered on refractory materials significantly impacts steel quality, production costs, and operational safety within steelworks. Consequently, numerous materials scientists have contributed to research on refractory applications by analyzing failure mechanisms and proposing mathematical models. For instance, Akkurt et al. demonstrated through high-temperature slag erosion tests on MgO–C bricks for tube furnaces, conducted under argon or CO atmosphere protection, that erosion intensifies with prolonged exposure and elevated temperatures. As the partial pressure of oxygen in the atmosphere increases and the alkalinity of the slag decreases, the erosion of refractory materials becomes more severe. The extent of slag erosion correlates with the rate of carbon loss.
Research indicates a linear relationship between the fractal dimension of the slag-eroded interface morphology and the refractory's resistance to slag erosion. In practice, the assessment of refractory damage and failure primarily relies on the experience and established practices of on-site technicians. During actual refining processes, the alkalinity of steel slag fluctuates. At present, the dynamic degradation process of ladle refractories over their service life until failure warrants further investigation. Therefore, this study employs an induction furnace rotary immersion method to investigate the effect of steel slag alkalinity on the erosion rate of magnesia–carbon bricks. It analyzes the degradation process of these bricks over time to simulate their operational deterioration. This provides practical guidance and theoretical reference for ensuring ladle safety, reducing refractory consumption, and enhancing clean steel quality.
Part 1: Testing
1. Sample Brick and Specimen Preparation
The sample brick used was a trapezoidal magnesia–carbon brick (upper section: 180 mm × 90 mm; lower section: 160 mm × 90 mm; height: 230 mm). Its physical and chemical properties were as follows: w(C) = 17%, bulk density = 2.87 g·cm⁻³, apparent porosity = 3.73%, and compressive strength at ambient temperature = 7.78 MPa. In the laboratory, the magnesia–carbon bricks were cut into test specimens measuring 45 mm × 45 mm × 230 mm using a cutting machine.
2. Test Procedure
The specimen was clamped in the test fixture. Approximately 15 kg of HRB400-grade rebar was loaded into the induction furnace. Power was applied for a 10-minute preheating period, after which the power was increased until the steel melted. Two types of refined steel slag, each weighing 200 g, were then measured and added to the furnace.
The furnace power was adjusted, and the surface temperature of the slag was measured using an infrared thermometer (model Ircon UX60P). When the surface temperature reached and stabilized at 1600°C, the specimen-securely clamped in the testing machine-was immersed into the molten steel within the induction furnace. Immersion was halted 15 cm above the base of the specimen (see schematic in Figure 1). Subsequently, the rotational speed switch of the induction furnace was activated to stabilize the specimen's rotational speed at 30 r·min⁻¹.
Refined steel slag 1 had an alkalinity of 1.3, while refined steel slag 2 had an alkalinity of 2.1. Their specific chemical compositions are shown in Table 1.


During the test, 50 g of refined slag was added to the induction furnace every 2 hours to maintain a stable slag composition and a constant temperature within the furnace. The erosion times were set at 0.5, 1, 1.5, 2, 2.5, 3, and 3.5 hours, respectively.
3. Performance Characterisation
Considering cutting tolerances and the uncertainty of the slag line layer, the four faces of each specimen were labeled A, B, C, and D, respectively. The width at every 1 cm interval from the lower base surface was measured and recorded using a steel ruler and a vernier caliper.
The damage index was used to characterize the extent of damage to the magnesia–carbon brick. This index represents the difference in width at the same height before and after the erosion test. For example, when the slag line layer of an eroded specimen is located 10 cm from the base, the original width at 10 cm on Face A (before erosion) is subtracted from the width after erosion. This difference corresponds to the total width loss of Face A, as erosion occurs simultaneously on both sides of the specimen face. Dividing this value by 2 yields the average width loss on Face A, which is defined as its damage index.
The same calculation is performed for the remaining three faces at the 10 cm mark to obtain the damage indices for all four faces. The sum of these four values, divided by four, gives the average damage index at the 10 cm height, representing the overall destruction index at that level. A schematic illustration of this calculation process is shown in Figure 2.

The degree of specimen damage is represented by the damage index y. In Figure 2, H₁ denotes the height of a specific position relative to the specimen base; different values of H₁ correspond to different slag line sections. The subscript i represents the surface at this height (i = 1 for surface A, i = 2 for surface B, and i = 3 and i = 4 for surfaces C and D, respectively). b denotes the specimen's width before erosion, while b′ denotes the width after erosion. The damage index is calculated using the formula shown in Equation (1):

Part 2: Results and Analysis
1. Erosion Analysis
The damage indices at the 10 cm mark of specimens subjected to erosion by Refined Steel Slag 1 and Refined Steel Slag 2 were calculated and plotted in Figure 3. Based on the relationship between the damage index and erosion time, the erosion rate was calculated as v=Δy/Δt, where Δy is the absolute difference in the damage index between two consecutive points, and Δt is the absolute difference in time between those points. The erosion rate was calculated for each pair of consecutive points, and the corresponding values for the two types of steel slag were plotted to form the curve shown in Figure 4.

As shown in Figure 3, the damage indices of magnesia–carbon bricks exposed to the two types of steel slag with differing alkalinity exhibit similar temporal patterns: they initially increase, then stabilize, and subsequently rise again. The lower-alkalinity Refined Steel Slag 1 stabilized first, at 1.5 hours. Comparing the damage indices over the same time periods shows that the damage index for low-alkalinity Refined Steel Slag 1 is consistently higher than that of high-alkalinity Refined Steel Slag 2. This indicates that low-alkalinity Refined Steel Slag 1 causes more severe damage to the magnesia–carbon bricks.

As shown in Figure 4, between 0.5 and 1.5 hours and between 2.5 and 3.5 hours, the erosion rate of magnesia–carbon bricks by low-alkalinity steel slag was greater than that by high-alkalinity steel slag. Between 1.5 and 2.5 hours, although the erosion rate of low-alkalinity steel slag was slightly lower than that of high-alkalinity steel slag, Figure 3 indicates that this interval represents a relatively stable erosion phase. However, for durations less than 2.5 hours, the damage index of low-alkalinity slag still exceeds that of high-alkalinity slag, indicating that the overall erosion effect of low-alkalinity slag is higher within the same timeframe. This confirms that low-alkalinity slag exhibits a higher erosion rate on magnesia–carbon bricks than high-alkalinity slag.
Analysis suggests that increased slag alkalinity elevates the calcium oxide (CaO) and magnesium oxide (MgO) content within the slag. These oxides neutralize certain acidic oxides in the magnesia–carbon brick, thereby reducing the saturation levels of CaO and MgO in the slag. This, in turn, diminishes the slag's dissolution effect on the aggregate within the magnesia–carbon brick.
The relationship between the CaO/SiO₂ mass ratio and phase composition in magnesia refractories indicates that when the CaO/SiO₂ mass ratio is ≥ 1.87, the formation of high-refractoriness minerals prevents a significant reduction in refractoriness. Following oxidation of carbon in magnesia–carbon bricks, the interface between steel slag and the bricks forms a MgO–CaO–SiO₂ phase. This corresponds to the formation of low-melting-point CMS compounds when the CaO/SiO₂ ratio is 0.93–1.87, and high-melting-point C₂S compounds when the ratio is ≥ 1.87. Refined Steel Slag 1 exhibits an alkalinity between 0.93 and 1.4, resulting in a higher proportion of low-melting-point CMS. This promotes the dissolution of magnesia particles, thereby accelerating their detachment.
2. Phase and Microstructural Analysis
The XRD pattern of the 10 cm surface of the refined steel slag erosion specimen is shown in Figure 5. Figure 5 demonstrates that erosion by low-alkalinity steel slag produces low-melting-point CMS. The presence of this low-melting-point substance promotes the dissolution of magnesia particles, thereby accelerating particle detachment.

The SEM image of the magnesia–carbon brick specimen after erosion by steel slag at the 10 cm position is shown in Figure 6. As shown in Figure 6(a), the interface between the steel slag and the magnesia–carbon brick is clearly visible, with noticeable penetration of the slag into the brick surface. This may be attributed to pores formed by the oxidation of surface carbon or to the presence of larger inherent surface pores, which facilitate the ingress of the steel slag. Figure 6(b) shows that the magnesia–carbon brick is not very dense, with substantial voids between particles. These voids provide space for steel slag to penetrate and erode the magnesia–carbon brick, thereby accelerating its oxidation.

To further confirm the presence of CMS, a sample eroded by Refined Steel Slag 1 at the 10 cm position was examined using scanning electron microscopy (SEM; see Figure 7) and energy-dispersive spectroscopy (EDS).

SEM images reveal that the eroded region contains numerous small particles, with larger particles exhibiting interconnected surface cracks. These fissures create pathways between the eroded area and the external environment, thereby accelerating carbon oxidation. Micro-area energy-dispersive spectroscopy (EDS) analysis at point 1 (x) showed the following composition: C 46.36%, O 37.41%, Mg 4.08%, Al 2.31%, Si 4.83%, Ca 5.01%. This confirms the formation of CaMgSiO₄ within the erosion zone.
Part 3: Conclusions
(1)For exposure times under 3.5 hours, low-alkalinity steel slag exhibits a higher erosion rate on magnesia–carbon bricks and also shows a greater damage index over the same period.
(2)Under alkalinity levels of 1.3 and 2.1, the erosion rate of steel slag on magnesia–carbon bricks follows the same pattern: increase → decrease → stabilization → increase.
(3)Low-melting-point compounds (CMS) are formed at the erosion interface of low-alkalinity steel slag. The presence of these compounds promotes the dissolution of magnesia particles, thereby accelerating their detachment.