Converter Longevity Code: 10 Key Technical Questions and Answers on Refractory Selection and Furnace Lining Life Extension
Converters are classified as acid or alkaline based on refractories, top-blown, bottom-blown, or side-blown according to the gas blowing position, and as air or oxygen converters based on the gas type. Alkaline oxygen top-blown and top-bottom double-blown converters are the most commonly used steelmaking equipment today, owing to their high production speed, large output, high single-furnace yield, low cost, and low investment. Converters are primarily used for producing carbon steel, alloy steel, and smelting copper and nickel.
01 What is the lining composition of a converter and what kind of refractory is built in each part?
The lining of a converter consists of an adiabatic layer (also known as a thermal insulation layer), a permanent layer, and a working layer.
The adiabatic layer is generally constructed using polycrystalline refractory fibers; the cap of the adiabatic layer is also sometimes rammed with resin-bonded magnesia. The bricks used in each part of the permanent layer are not entirely the same, and it is mostly constructed with low-grade magnesia-carbon bricks, tar-bonded dolomite bricks, or sintered magnesia bricks. The entire working layer is constructed with magnesia-carbon bricks.
02What is an integrated furnace lining?
With integrated masonry, the erosion degree of the entire furnace lining bricks is more balanced, which can extend the overall service life of the furnace.
(1) Furnace mouth part: It should be constructed with magnesia-carbon bricks that have high thermal shock resistance, good slag resistance, resistance to scouring by slag and high-temperature furnace gas, and are not prone to sticking to steel; even if steel does stick, it can be easily cleaned.
(2) Furnace cap part: It should be constructed with magnesia-carbon bricks that have good thermal shock resistance and slag resistance.
(3) Lining bricks on the charging side: In addition to high slag resistance and high-temperature strength, they should also have good thermal shock resistance. Generally, magnesia-carbon bricks with added antioxidants are used for construction.
(4) Lining bricks on the tapping side: They are less affected by thermal shock but are subject to thermal shock from molten steel and scouring effects. Magnesia-carbon bricks of the same grade as those used on the charging side are often employed, but their thickness can be slightly reduced.
(5) Brick linings on both sides of the trunnion: In addition to erosion during the blowing process, their surfaces are not covered by a slag layer, so the carbon in the brick linings is easily oxidized. This area is difficult to repair, leading to more severe erosion.
(6) Brick linings in the slag line area: This part is in prolonged contact with slag and is subject to severe slag erosion. The slag line on the tapping side changes with tapping time and is less distinct. However, the slag line on the other side, due to intense slag erosion combined with other forces acting on the converter belly during the blowing process, undergoes more severe erosion under the combined effect of these two factors.
(7)Molten pool part: Also known as the furnace cylinder and furnace bottom. During the blowing process, although it is subject to erosion by molten steel, the damage is less severe compared to other parts.
03 What kind of refractory bricks are built in the outlet and what are the two ways of replacing them?
The taphole is severely damaged due to erosion by high-temperature molten steel and the impact of drastic temperature changes. Therefore, it should be constructed using magnesia-carbon bricks with good erosion resistance and high oxidation resistance.
There are two methods for replacing the taphole: one is complete replacement; the other is rebuilding the taphole. To rebuild the taphole, first clean out the original taphole, then insert a steel pipe whose inner diameter matches the size of the taphole. After that, fill the area around the outer wall of the steel pipe with ramming mass and sinter it.
04 What are the requirements for the masonry of furnace lining bricks?
The masonry quality of a converter furnace lining is the foundation for its service life. Therefore, first, the quality of the furnace lining bricks themselves must comply with standard regulations; second, masonry must be carried out in strict accordance with technical operating procedures to meet the requirements of overall quality standards.
(1) The working layer should use integrated furnace masonry.
(2) Masonry must follow the principles of "tight fitting, solid backing, and thorough filling." Bricks should fit as tightly as possible to each other, with vertical brick gaps ≤1mm and small-section top-bottom gaps ≤2mm. However, a certain number of expansion joints must be reserved. Joints and gaps should be filled with refractory filler materials and tamped tightly. The space between the insulation layer and permanent layer, and between the permanent layer and working layer, should be solidly filled with magnesia sand.
(3) The masonry of the furnace bottom must ensure levelness.
(4) The position of brick masonry joints should be selected appropriately. Joint bricks should use adjusting bricks or cut bricks, and must be tightly braced. Brick joints should be staggered layer by layer, with uniform offsets at each section.
(5) The working layer should use dry masonry, while the taphole may use wet masonry. The taphole must be installed and constructed in strict accordance with technical specifications.
(6)The joint between the furnace bottom and furnace body must be tight to prevent steel leakage.
05 What is the mechanism of erosion of magnesia-carbon bricks in the working layer of a converter lining?
The working layer of a converter lining is made of magnesia-carbon bricks. Magnesia-carbon bricks contain a considerable amount of graphite, which has poor wettability with slag. This hinders the penetration of slag into the brick body, thus extending the service life of magnesia-carbon bricks.
The erosion mechanism of magnesia-carbon bricks is as follows:
Observations of residual magnesia-carbon bricks reveal that their working surface is relatively smooth but has a distinct three-layer structure. The working surface features a very thin (1–3mm) slag penetration layer, also known as the reaction layer. Adjacent to the reaction layer is a decarburized layer (0.2–2mm thick), also called the altered layer, which is adjacent to the original brick layer. The chemical composition and petrographic structure of each layer differ.
Carbon on the working surface of magnesia-carbon bricks is first oxidized by oxidizing components such as TFe in the slag, as well as oxidizing atmospheres (O₂, CO₂, etc.) in the furnace gas, and by the reduction of MgO at high temperatures. This oxidation leads to the formation of a decarburized layer on the working surface of the magnesia-carbon bricks. The reaction formulas are as follows:
FeO + C → CO↑ + Fe
CO₂ + C → 2CO↑
MgO + C → Mg + CO↑
Due to the oxidation and removal of carbon from the working surface of the brick, the brick's structure becomes loose and brittle. It then erodes under the scouring action of the molten bath. As the reaction continues, low-melting-point compounds accumulate, gradually reducing the viscosity of the liquid bonding phase until it can no longer bind the magnesia grains and aggregate particles. This causes the ablation of magnesia grains and the dissolution of magnesia particles, which then separate and float into the slag, increasing the brick's melt loss over time. As the slag penetration layer (altered layer) erodes, the decarburized layer becomes the new slag penetration layer, and a fresh decarburized layer forms adjacent to the original brick layer. The brick is damaged by melting due to the combined effect of these processes.
Magnesia-carbon bricks undergo oxidation → decarburization → erosion, eventually causing magnesia particles to be lost to the slag. This is how magnesia-carbon bricks are eroded and damaged. It follows that improving the oxidation resistance of the bricks is key to extending their service life.
06 What methods are used to maintain the converter lining in daily production?
Slag splashing for furnace protection is the primary method for maintaining the furnace lining in daily production. Additional maintenance methods are determined based on the location and extent of lining brick erosion. Generally, the furnace lining is maintained using patching materials or repair bricks, along with spraying and patching techniques, to maintain a reasonable internal shape of the converter.
For example, furnace bottom maintenance primarily involves patching. Based on the residual brick thickness measured by a laser gauge, the amount of patching material and baking time are determined. Magnesium-based cold patching materials or repair bricks are used for this purpose. The charging side of the furnace body can be maintained using a combination of spray patching and patching materials. The trunnion and slag line areas can only be maintained by spray patching. Depending on the extent of damage, the taphole is either completely replaced or repaired with patching materials. Under normal slag splashing conditions, the furnace cap does not require spray patching, but it can be spray-patched if necessary.
07 Under what circumstances is the spray-patching technique used for the converter lining?
The furnace lining uses the spray-patching technique when there is localized damage that is unsuitable for repair with patching materials, such as damage to the trunnion parts. Refractory material is sprayed intensively onto areas with severe local erosion, allowing it to sinter with the lining bricks and repair the furnace lining.
Spray-patching methods include dry spray-patching, semi-dry spray-patching, and flame spray-patching. Currently, semi-dry spray-patching materials are used most commonly.
08 Why does the spattered slag layer protect the furnace lining?
The slag adhesion layer spattered onto the furnace lining surface consists of various minerals. When the temperature rises, low-melting-point minerals melt first, separating from high-melting-point phases and gradually flowing down from the spattered slag layer into the high-temperature slag. The high-melting-point minerals remaining on the lining surface enhance the slag layer's high-temperature resistance-a phenomenon known as selective melting (or fractional melting). Meanwhile, the slag layer chemically reacts with the furnace lining refractories. Through the cyclic process of slag spattering → selective melting → re-spattering, a spattered slag layer gradually forms on the furnace lining surface.
It is inferred that after multiple cycles of spattering, selective melting, and re-spattering, the spattered slag layer has a significantly reduced content of low-melting-point compounds, with residual components consisting of high-melting-point minerals. This allows the spattered slag layer to protect the furnace lining.
09 What are the requirements for blowing the first heat after baking?
The blowing operation of the first heat is also known as commissioning a new furnace. Although the furnace lining has been baked for several hours, only the surface of the lining has accumulated some heat, and the overall temperature of the lining remains very low. Therefore:
(1) No scrap is added to the first heat, and only hot metal is charged.
(2) Based on the hot metal composition, hot metal temperature, and the materials to be added, heat balance calculations are performed to determine whether ferrosilicon (Fe-Si) or coke needs to be added to supplement heat.
(3) Slag-forming materials are added according to the hot metal composition.
(4) Due to the low temperature of the furnace lining, the taphole is small, and the tapping time is prolonged, so the tapping temperature should be approximately 20°C higher than that of normal blowing.
(5)Within the first 6 heats after commissioning a new furnace, steelmaking should be continuous, and no planned stoppages are allowed within the first 100 heats.
10 Why does the furnace bottom sometimes rise, and how can furnace bottom rise be prevented?
After the application of slag splashing furnace protection technology, the bottom of a converter is prone to rise. The main reason is that slag splashed with high alkalinity final slag-where the MgO content reaches or exceeds the saturation point-causes MgO crystals to precipitate as the furnace temperature drops after tapping. High-melting-point minerals like C₂S and C₃S also precipitate, increasing slag viscosity. Part of the splashed slag adheres to the furnace lining surface, while the remaining slag accumulates at the furnace bottom. This slag combines with magnesia crystals in the bottom magnesia-carbon bricks, causing the furnace bottom to rise. During repeated blowing and slag splashing, bottom gas supply and cold air from top-bottom blowing lower the furnace temperature, further increasing slag viscosity. High-melting-point crystals (C₂S, C₃S) grow and are surrounded by MgO crystals or solid particles, forming a hard, dense layer. Improper bottom gas supply exacerbates furnace bottom rise.
To avoid furnace bottom rise, the following measures should be taken:
(1) Control end-point slag composition and temperature to prevent excessive slag viscosity.
(2) Adopt an appropriate lower slag splashing gun position.
(3) Maintain sufficient nitrogen pressure and flow rate.
(4) Remove residual slag promptly after slag splashing.
(5) Optimize the slag splashing frequency.
(6) If furnace bottom rise exceeds the specified limit, use an oxygen lance to melt the rise or add appropriate amount of) Fe-Si to melt the elevated bottom.