What is the wear mechanism of magnesia-carbon bricks used for electric furnace linings?

 

Generally, magnesia-carbon bricks are made from high-quality magnesia clinker, mixed with high-purity graphite and additives such as silicon and silicon carbide, and pressed using phenolic resin as the binder. The basic requirements for magnesia-carbon bricks used in electric furnaces are as follows:

 

(1) Low thermal conductivity to ensure minimal heat loss and improve the thermal efficiency of the electric furnace;

 

(2) High resistance to thermochemical and thermophysical erosion, i.e., good volume stability;

 

(3) Excellent slag resistance, spalling resistance, oxidation resistance, and high compressive strength, thereby achieving low consumption and a long service life.

 

During the baking of a new furnace lining, the main reactions occur when the lining temperature reaches 750℃.

 

WPS1

 

Reaction 1 mainly involves the migration of generated magnesium vapor and carbon monoxide gas along the pores to the high-temperature zone. Reaction 2 describes the re-oxidation of magnesium vapor into magnesium oxide on the surface layer of the furnace wall, where it forms high-melting-point petrographic compounds with other trace components in the magnesia-carbon bricks. Therefore, controlling the heating schedule during furnace baking to prevent the extensive occurrence of Reaction 1 is the key to maintaining the volume stability of magnesia-carbon bricks. This is important for both converters and electric furnaces. The direct consequence of improper furnace baking is lining collapse or a significant reduction in lining service life, from which many domestic manufacturers have accumulated extensive experience and lessons.

 

What are the erosion mechanisms of electric furnace linings during normal service?

 

During normal smelting, the furnace lining is in direct contact with high-temperature molten steel and slag under extremely severe operating conditions. The main causes of lining damage are as follows:

 

(1) Thermal spalling caused by arc radiation and chemical erosion at high temperatures;

 

(2) Scouring action of molten slag, molten steel, and furnace gas on the furnace lining;

 

(3) Chemical corrosion of the furnace lining by molten slag;

 

(4) Spalling caused by temperature fluctuations;

 

(5) Layer cracking and other damage resulting from the decomposition of the mineral composition within the lining bricks themselves;

 

(6) Mechanical impact and scouring of the furnace lining during the charging of scrap steel and the addition of hot metal.

 

How does the erosion process of magnesia-carbon bricks occur during electric furnace smelting?

 

The basic erosion process of magnesia-carbon bricks is as follows:

 

(1) After reaction, magnesia-carbon bricks are divided into three layers: the original brick layer (the unreacted brick body), the decarburized layer (formed by the self-consumption reaction between internal MgO and carbon), and the dense layer (the part in contact with molten slag).

 

(2) Self-consumption reaction between MgO and carbon inside magnesia-carbon bricks at high temperatures:

 

WPS2

 

(3) Direct reaction with oxides in the slag:

(Fe₂O₃) in slag + C (in brick) = 2(FeO) + {CO}

 

Magnesium oxide is reduced to magnesium vapor, which migrates to the surface along the pores of the refractory and is re-oxidized to MgO. It then forms a high-viscosity petrographic structure with other impurity elements in the brick body, commonly referred to as the dense layer.

 

The erosion process is as follows:

 

(1) Physical wear: During the blowing process of the converter, the movement of molten slag and furnace gas causes mechanical wear and spalling of these petrographic structures into the slag.

 

(2) Chemical erosion: Various components in the slag react with the dense layer of the brick. Among them, FeO promotes the dissolution and transfer of magnesium oxide into the slag, thereby accelerating the erosion of magnesia-carbon bricks.

 

(3) Effect of temperature on erosion: Higher temperatures reduce the viscosity of the slag, intensify physical erosion, and deepen the decarburized layer, resulting in accelerated erosion. The relationship between the decarburized layer and brick temperature is shown in Figure 1.

 

WPS4

 

What is the approximate structure of the dense layer formed in magnesia-carbon bricks, and what effect does it have on slag resistance?

 

The reaction between magnesia-carbon bricks and molten slag forms a dense reaction layer (see Figure 2), which improves the slag corrosion resistance of the material. If a material has poor oxidation resistance, its microstructure will become loose after use, allowing molten slag to penetrate into the interior of the material, damage the original brick layer, and ultimately lead to complete failure of the material.

 

WPS5

 

Once the damage mechanism of refractory materials for electric furnace linings is understood, suitable, durable, and long‑service refractories can be selected accordingly.

 

The furnace wall of an electric furnace is generally lined with magnesia‑carbon refractories, while the furnace bottom is usually constructed with a ramming mix, mostly magnesia‑calcia dry ramming mix.

 

These materials must sinter rapidly, form a solid working layer, minimize molten slag penetration, and retain moderate porosity in the deeper layers.