Effects Of Curing Humidity On Demolding Strength Of CAC-Bonded Castables

Apr 02, 2026

Leave a message

 

Effects of Curing Humidity on Demolding Strength of CAC-Bonded Castables

 

CAC

 

Calcium aluminate cement (CAC) reacts with water under different curing conditions to form various hydrate phases (CAH₁₀, C₂AH₈, C₃AH₆, and AH₃). These hydrate phases differ in morphology and structure and can form an interlocking network, which contributes to the early strength of CAC-bonded castables. Owing to their high early strength, excellent corrosion resistance, and wear resistance, CAC-bonded castables are widely used not only in the concrete industry but also in high-temperature industrial applications, such as refining furnace lids, ladle supports, and cement kiln inlets.

 

The hydrate phases of CAC depend on the curing conditions. According to the literature, curing temperature, humidity, curing time, and the type and content of micropowders significantly influence the hydration products of calcium aluminate cement, thereby affecting the properties and microstructure of corundum castables.

 

At present, few studies have reported on the effect of curing humidity on the demolding strength of castables and the underlying mechanisms. Some researchers suggest that curing CAC-bonded castables under high humidity provides sufficient moisture to promote CAC hydration, which may lead to higher strength. However, in practical production, some believe that curing castables at relatively high temperatures and low humidity results in even higher strength despite the reduced amount of free water. Furthermore, it remains unclear whether the difference in demolding strength between high- and low-humidity curing is caused by variations in the hydrate phases after curing, which requires further investigation.

 

Accordingly, this study investigates the effects of high and low curing humidity on the hydrate phases of CAC and the demolding strength of CAC-bonded castables and analyzes the mechanisms by which curing humidity influences the demolding strength of the castables.

 

Experiments

 

1.1 Raw Materials

 

The raw materials used in the experiments included tabular alumina aggregates and fine powders with w(Al₂O₃) ≥ 99.3% (particle sizes: 6–3 mm, 3–1 mm, 1–0.5 mm, ≤0.5 mm, and ≤0.045 mm), bimodal activated α-alumina micropowder with w(Al₂O₃) ≥ 99.6% (CL370, d₅₀ = 2.2 μm), pure CAC cement (Secar-71), and the dispersants DC1 and DH1.

 

1.2 Specimen Preparation

 

For the preparation of castable specimens, the batched raw materials were first mixed in a mixer for 30 s. Water was then added, and mixing was continued for 180 s, followed by vibration casting to form green specimens with dimensions of 40 mm × 40 mm × 160 mm. The green bodies were cured at 50 °C under two different humidity conditions (RH = 30% and RH = 80%).

 

In addition, to observe the hydrate phases at different curing times, the curing durations were set to 3 h, 6 h, 12 h, and 24 h. The demolding strength was tested after curing and demolding. The formulation of the CAC-bonded castables is listed in Table 1.

 

1

 

Furthermore, to investigate the phase and structural changes of cement hydration products under different curing humidities, matrix specimens were prepared using CAC cement and alumina micropowder.

 

According to a mass ratio of alumina micropowder to calcium aluminate cement of 6:4, 12 g of alumina micropowder and 8 g of CAC cement were weighed, placed into plastic cups, and mixed uniformly.

 

Tap water was added at a water–solid ratio (mass ratio of water to solid) of 1, followed by stirring for 10 min until a homogeneous mixture was obtained.

 

The matrix specimens were kept in plastic cups with a diameter of approximately 44 mm and a thickness of about 15 mm.

 

The matrix samples were cured under the same conditions as the castables.

 

The matrix formulation is listed in Table 2.

 

2

 

1.3 Properties Testing

 

The cold modulus of rupture (CMOR) and cold compressive strength (CCS) of the castables after demolding at room temperature were tested in accordance with GB/T 3001-2007 and GB/T 5072-2008.

 

The cured matrix specimens were subjected to freeze-drying (temperature: −30 °C; duration: 24 h). Subsequently, X-ray diffraction (XRD) and scanning electron microscopy (SEM) were used to analyze the phase composition and microstructural characteristics of the freeze-dried specimens, respectively.

 

Results and Discussion

 

Figure 1 shows the modulus of rupture and compressive strength of CAC-bonded castables after demolding, following curing at different humidities (RH = 30% and RH = 80%) for various durations from 3 h to 24 h.

 

At the same curing time, both the modulus of rupture and compressive strength of the castables cured at lower humidity (RH = 30%) were higher than those cured at higher humidity (RH = 80%). As the curing time increased from 3 h to 24 h, the demolding strength of the castables under both curing humidities showed a continuous increase.

 

WPS1

 

Figure 2 shows the XRD patterns of the matrix specimens after freeze-drying under two curing humidity conditions.

 

WPS2

 

It can be seen from Figure 2(a) that the matrix specimens cured at 50 °C and RH = 30% exhibit the same phase composition after different curing durations, consisting of α‑Al₂O₃, C₂AH₈, and AH₃. Under these curing conditions, the castable loses considerable moisture during curing, resulting in insufficient water for hydration. With limited water, the C₂AH₈ phase initially formed by CAC hydration cannot transform into C₃AH₆ and AH₃ via the dissolution–precipitation mechanism, so C₂AH₈ and AH₃ remain the main hydrate phases after low-humidity curing.

 

Figure 2(b) shows that, in addition to α‑Al₂O₃, C₂AH₈, and AH₃, a new hydration product, C₃AH₆, appears after different curing times. This is attributed to the relatively low water loss of the castable during high-humidity curing. Under sufficient free water conditions, the C₂AH₈ phase formed in the early stage of hydration gradually transforms into C₃AH₆ and AH₃ through the dissolution–precipitation mechanism.

 

Figure 3 shows the microstructures of matrix specimens freeze-dried after curing at RH = 30% for 12 h and 24 h. The hydration products in the castable matrix cured at RH = 30% are C₂AH₈ and AH₃. The SEM results are consistent with the XRD analysis and also in agreement with the findings of Wang Xiaoyu. Plate-like hydrate phase C₂AH₈ and fine granular hydration product AH₃ can be clearly observed in the SEM micrographs.

 

WPS3

WPS4

 

As the curing time is extended, more plate-like and interlocking hydrate phases of C₂AH₈ can be observed, and the distribution of C₂AH₈ becomes more uniform. This indicates that the plate-like hydrate product C₂AH₈ forms a networked interlocking structure by intersecting with itself, while also encapsulating the granular hydrate product AH₃. The packing between different components becomes denser, thereby enhancing the demolding strength of the castables (see Figure 1).

 

Figure 4 shows the microstructures of the matrix specimens cured at a relative humidity of RH = 80% for 12 h and 24 h.

 

WPS5

WPS6

 

It can be clearly seen from the SEM micrographs that large granular hydration product C₃AH₆ appears in the matrix after high‑humidity curing. This observation is consistent with the XRD pattern shown in Figure 2(b).

 

After curing at a relative humidity of RH = 80% for 12 h, the matrix contains granular hydration products C₃AH₆ and AH₃, as well as a small amount of plate‑like C₂AH₈. When the curing time is extended to 24 h, a considerable amount of C₃AH₆ is formed in the matrix, and almost no plate‑like C₂AH₈ can be observed. This occurs because the specimens retain abundant moisture under high‑humidity curing, allowing the initially formed C₂AH₈ to further transform into C₃AH₆ and AH₃ via the dissolution–precipitation mechanism.

 

The images also show large voids between the granular hydration product C₃AH₆ and the internal hydration products, as well as among various components within the specimen. These voids contribute to the lower demolding strength of the specimens cured under high‑humidity conditions (RH = 80%), as shown in Figure 1.

 

In summary, differences in curing humidity lead to variations in hydration products, resulting in different demolding strengths of castables. Under low‑humidity curing (RH = 30%), the hydrate phases are C₂AH₈ and AH₃, whereas under high‑humidity curing (RH = 80%), the main hydrate phases are C₃AH₆ and AH₃.

 

The structure and morphology of C₂AH₈ and C₃AH₆ are completely different. In specimens cured at low humidity, plate‑like C₂AH₈ forms an interlocking network, whereas under high humidity, it transforms into discrete granular C₃AH₆, resulting in lower demolding strength of the castables.

 

Additionally, the bulk density of C₂AH₈ (1.95 g/cm³) is lower than that of C₃AH₆ (2.52 g/cm³). The voids between the granular C₃AH₆ and internal hydration products, as well as among various components, increase significantly. This further contributes to the lower demolding strength of specimens cured at high humidity (RH = 80%) compared with those cured at low humidity (RH = 30%).

 

Conclusion

 

(1)At a curing temperature of 50 °C, CAC‑bonded castables cured at high humidity (RH = 80%) exhibit lower demolding strength than those cured at low humidity (RH = 30%).

 

(2)When cured at 50 °C and RH = 30%, the initially formed hydrate phase C₂AH₈ cannot transform into C₃AH₆ and AH₃ through the dissolution–precipitation mechanism due to insufficient water, resulting in C₂AH₈ and AH₃ remaining as the final hydrate phases. In contrast, under higher curing humidity (RH = 80%) with sufficient free water, most C₂AH₈ is converted into C₃AH₆ and AH₃ via the dissolution–precipitation mechanism, making C₃AH₆ and AH₃ the dominant hydrate phases.

 

(3)The plate‑like C₂AH₈ formed under low humidity develops an interlocking network structure, which provides demolding strength to the castables. By comparison, the granular hydration product C₃AH₆ formed under high humidity has a higher bulk density and forms a loose structure with large voids between itself and other hydration products as well as among components, resulting in reduced castable strength.