Erosion Resistance Of Tabular Alumina, Activated Alumina Powder, And Magnesia-Alumina Spinel Powder in Low-Carbon Magnesia-Carbon Bricks

Nov 17, 2025

Leave a message

 

Erosion Resistance of

Tabular Alumina, Activated Alumina Powder, and Magnesia-Alumina Spinel Powder

in Low-Carbon Magnesia-Carbon Bricks

 

Magnesia-carbon bricks are composite materials prepared using high-melting-point basic oxide magnesium oxide and graphite (which is hardly wetted by slag) as the main raw materials, supplemented with binders (such as phenolic resin), antioxidants, and other additives. They are widely used in key areas such as the linings and slag lines of converters and ladles, as well as in the linings of AC and DC electric arc furnaces. To maximize the performance of magnesia-carbon bricks, the design of their microstructure is crucial. Taking into account the properties of the raw materials and their structural compatibility, the main design principles are as follows:

 

(1) Design the particle size distribution in accordance with the principle of closest packing to obtain highly dense magnesia-carbon bricks;

 

(2) In addition to coating the surface of magnesia particles, graphite should also be partially distributed in the matrix to reduce the penetration of molten slag into the matrix and the erosion along periclase grain boundaries, thereby decreasing damage to the magnesia-carbon bricks;

 

(3) Use graphite and other substances to coat the surface of magnesia aggregates to alleviate the expansion stress of the aggregates;

 

(4) The distribution of antioxidants should be as compatible as possible with that of graphite and phenolic resin.

 

With the continuous development of new-generation high-quality steel grades such as clean steel, the requirements for magnesia-carbon bricks used in converters, ladles, and other equipment have become increasingly stringent. To avoid increasing the carbon content in molten steel, low-carbon or ultra-low-carbon magnesia-carbon bricks have become a focus of research in recent years. For low-carbon magnesia-carbon bricks (with a carbon mass fraction not exceeding 8%) or ultra-low-carbon magnesia-carbon bricks (with a carbon mass fraction not exceeding 3%), the carbon content is insufficient to form a continuous carbon network. Compared with traditional magnesia-carbon bricks with a carbon mass fraction of 10% to 20%, these materials suffer from problems such as poor resistance to molten slag penetration. Studies have reported that low-carbon magnesia-carbon bricks can be prepared through graphite compounding, but the penetration resistance and erosion resistance of the resulting materials still do not meet the requirements of smelting processes. Therefore, designing the microstructure of low-carbon magnesia-carbon bricks is crucial for developing high-performance low-carbon and ultra-low-carbon refractory materials.

 

To optimize the microstructure and performance of low-carbon magnesia-carbon bricks, Al₂O₃ is introduced into the low-carbon magnesia-carbon matrix. The properties of alumina and its high-temperature reactions are utilized to compensate for the performance deficiencies caused by low carbon content. The introduction of Al₂O₃ into low-carbon magnesia-carbon materials serves two functions: first, the micro-volume expansion produced by the formation of magnesia-alumina spinel from Al₂O₃ at high temperatures improves the microstructure and increases the density of the material, thereby reducing porosity and enhancing resistance to molten slag penetration; second, the formation of magnesia-alumina spinel at high temperatures improves the erosion resistance of low-carbon magnesia-carbon materials. However, the form in which Al₂O₃ is introduced has a significant effect on the microstructure and service performance of low-carbon magnesia-carbon bricks.

 

To determine the suitable form of Al₂O₃ introduction for ultra-low-carbon magnesia-carbon bricks, this study investigates the use of α-Al₂O₃ micropowder, tabular alumina powder, and spinel fine powder as additives. The findings provide a reference for the microstructure design and performance optimization of low-carbon and ultra-low-carbon magnesia-carbon bricks.

 

01 Experimental Section

 

1.1 Raw Materials

 

The raw materials used in the experiment were as follows:

Fused magnesia particles with particle sizes of 3–5 mm, 1–3 mm, and 0–1 mm, and fused magnesia fine powder with a particle size of less than 0.088 mm. Its chemical composition (mass fraction, w/%) was: MgO 97.50; SiO₂ 0.61; CaO 1.39; Fe₂O₃ 0.63.

Graphite with a particle size of less than 0.15 mm and a carbon (C) mass fraction of 96.41%.

Aluminum (Al) powder with a particle size of less than 0.074 mm and an Al mass fraction of 98.52%.

Silicon (Si) powder with a particle size of less than 0.074 mm and an Si mass fraction of 98.21%.

α-Al₂O₃ micropowder with a D50 of 1.2 μm and an Al₂O₃ mass fraction of 99.25%.

Fused magnesia–alumina spinel powder with a particle size of less than 0.088 mm. Its chemical composition (mass fraction, w/%) was: MgO + Al₂O₃ ≥ 98.5; MgO 22–28; Al₂O₃ 71–77; K₂O + Na₂O ≤ 0.3; Fe₂O₃ ≤ 0.3.

Tabular alumina powder with a particle size of less than 0.088 mm and an Al₂O₃ mass fraction of more than 98%.

Thermosetting phenolic resin was used as the binder.

 

1.2 Preparation of Magnesia-Carbon Brick Samples

 

The experimental scheme for preparing the magnesia-carbon brick samples is shown in Table 1. According to the scheme in Table 1, the required raw materials were weighed and mixed in a small wet mill for 10 minutes, following the mixing method used for magnesia-carbon bricks at construction sites. The mixed material was formed using a hydraulic press under a forming pressure of 200 MPa, with final dimensions of 155 mm × 50 mm × 50 mm. The formed samples were dried at 200 °C for 24 hours and then placed in a high-temperature furnace for buried-carbon sintering at 1580 °C for 3 hours. After sintering, the samples were cooled together with the furnace.

 

WPS1

 

The static crucible method was used to test the slag erosion resistance of the samples. Three blind holes with dimensions of φ35 mm × 35 mm were drilled in the unsintered samples, and equal amounts of steel slag were added. The chemical composition of the steel slag (mass fraction, w/%) was: SiO₂ 3.68; Al₂O₃ 38.00; Fe₂O₃ 13.10; CaO 27.83; MgO 9.53; Cr₂O₃ 0.65. Note: The duplicate "MgO" in the original text is retained as provided; it is recommended to verify the actual composition, as it is likely a typo for another oxide such as TiO₂ or MnO₂. The samples containing steel slag were placed in a high-temperature furnace and held at 1580 °C for 2 hours. X-ray diffraction (XRD) and scanning electron microscopy (SEM) were used to analyze the phase composition and microstructure of the samples after the reaction.

 

1.3 Characterization

 

The bulk density and apparent porosity of the samples were measured in accordance with the GB/T 2997-2015 standard.

The phase composition of the samples was analyzed using a D8 Advance X-ray diffractometer manufactured by Bruker (Germany).

The microstructure of the samples was observed using an SU8200 scanning electron microscope produced by Hitachi (Japan).

 

02 Results and Discussion

 

2.1 Phase Analysis

 

The XRD patterns of the sintered samples from Groups B to G are shown in Figure 1.

 

WPS2

 

It can be observed from Figure 1 that after high-temperature treatment, a magnesia-alumina spinel phase exists in all samples, regardless of the form in which Al₂O₃ was added. This indicates that both tabular alumina powder and α-Al₂O₃ micropowder react with magnesia powder at high temperatures to form magnesia-alumina spinel.

 

2.2 Porosity and Microstructure Analysis

 

The porosity of the sintered samples from Groups A to H is shown in Table 2.

 

WPS3

 

It can be observed from Table 2 that, compared with the blank sample A and the samples containing fused spinel, the samples with tabular alumina or α-Al₂O₃ micropowder exhibit lower porosity after sintering. This indicates that the micro-expansion effect during spinel formation can further reduce porosity and improve the penetration resistance of the samples. In contrast, for samples D and E, which contain directly added fused spinel fine powder, the porosity only slightly decreases, showing minimal change because no reactive spinel formation occurs. Samples F and G, which were added with α-Al₂O₃ micropowder, have the lowest porosity, indicating a relatively strong micro-expansion effect from the spinel formed and demonstrating that α-Al₂O₃ micropowder promotes spinel formation. The SEM images of the samples after heat treatment are shown in Figure 2.

 

WPS4

a – Blank sample A; b – Sample G with 6% α-Al₂O₃ micropowder added; c – Sample C with 6% tabular alumina added; d – Sample E with 6% magnesia-alumina spinel added.

 

As shown in Figure 2, the intergranular pores of the blank sample A are significantly larger (Figure 2a). Sample G, with α-Al₂O₃ micropowder added, exhibits relatively dense intergranular gaps (Figure 2b). The intergranular compactness of Sample C, with tabular alumina added (Figure 2c), is lower than that of Sample G but higher than that of Sample E, with directly added magnesia-alumina spinel (Figure 2d).

 

Due to the good dispersibility and large specific surface area of α-Al₂O₃ micropowder, which promotes the spinel formation reaction, the porosities of Samples F and G with α-Al₂O₃ micropowder are both lower than those of Samples B and C with tabular alumina (Table 2). The intergranular compactness of the samples with added magnesia-alumina spinel is lower than that of the samples with added tabular alumina and slightly higher than that of the blank sample A, indicating that Samples D and E, with spinel fine powder added, contribute little to reducing the porosity of the magnesia-carbon material after heat treatment.

 

2.3 Analysis of Slag Erosion Resistance

 

The hole expansion rate of the samples after slag erosion is shown in Table 3.

 

WPS5

 

As shown in Table 3, Sample H (conventional magnesia-carbon brick) exhibits the best slag erosion resistance. Owing to its relatively high graphite content, it demonstrates excellent resistance to molten slag erosion. In contrast, Sample A (low-carbon magnesia-carbon brick without any additives) shows the poorest slag erosion resistance, with a significantly higher hole expansion rate. Among the samples with α-Al₂O₃ micropowder, Sample G (6% α-Al₂O₃ micropowder) has a larger hole expansion rate than Sample F (4% α-Al₂O₃ micropowder), indicating that its matrix phase has inferior erosion resistance.

 

According to relevant literature, intragranular spinel formed at MgO grain boundaries during cooling can effectively enhance material densification, thereby improving resistance to molten slag penetration. However, the service conditions of magnesia-carbon bricks are complex, especially under the oxygen-rich and calcium-rich environment of converter smelting. Magnesia-alumina spinel tends to form composite spinel with FeOₓ, while free α-Al₂O₃ micropowder may react with CaO in the slag to form C₃A (tricalcium aluminate, melting point: 1535 °C), a low-melting phase that reduces slag erosion resistance. Therefore, despite the relatively dense microstructure of Sample G (6% α-Al₂O₃ micropowder), its slag erosion resistance still does not meet practical requirements compared with other samples.

 

The slag erosion resistance of a material depends not only on chemical reactions with molten slag but also on slag penetration behavior. Among all low-carbon samples, Sample F (4% α-Al₂O₃ micropowder) exhibits the best slag erosion resistance, outperforming Sample A, Sample G, and other low-carbon counterparts. This is attributed to the formation of magnesia-alumina spinel, which enhances sample compactness, reduces carbon oxidation, and improves penetration resistance. The excellent penetration resistance limits slag penetration depth and weakens the reaction between the material and molten slag, thereby improving erosion resistance.

 

In summary, adding 4% α-Al₂O₃ micropowder to low-carbon magnesia-carbon bricks enhances their slag erosion resistance. Tabular alumina was selected as an additive due to its high Al₂O₃ purity; fused magnesia-alumina spinel powder was chosen for its high purity, high melting point (2135 °C), and volume stability at elevated temperatures; and active α-Al₂O₃ micropowder was adopted for its high purity and relatively large specific surface area, facilitating in-situ spinel formation.

 

As shown in Table 3, the hole expansion rates of Samples B–E (added with tabular alumina or fused spinel) are all higher than those of Samples F–G (added with α-Al₂O₃ micropowder). This is because: (1) the Al₂O₃ purity of tabular alumina (98%) is lower than that of α-Al₂O₃ micropowder, and its particle size (0.088 mm) is much larger than the 1.2 μm of α-Al₂O₃ micropowder, which hinders in-situ magnesia-alumina spinel formation; (2) although Samples D–E (added with fused magnesia-alumina spinel) show relatively good slag resistance due to the high purity of the pre-synthesized spinel, the lack of an in-situ spinel formation reaction at high temperatures prevents micro-volume expansion, so micro-porosity is not reduced.

 

Further microstructure analysis of the samples was conducted using a scanning electron microscope, and the results are presented in Figure 3.

 

WPS6

a - Blank sample A; b - Conventional magnesia-carbon brick; c - Sample with 4% α-Al₂O₃ micropowder added; d - Sample with 6% α-Al₂O₃ micropowder added; e - Sample with 6% tabular alumina added; f - Sample with 6% magnesia-alumina spinel added.

 

As can be seen from Figure 3, the blank sample A exhibits the poorest penetration resistance, with molten slag penetrating deeply into the material. The conventional magnesia-carbon brick (Sample b) has the thinnest slag penetration layer (only a few tens of micrometers). This is because the graphite in the material reduces the iron oxides in the infiltrated steel slag, thereby altering the slag's composition and properties and significantly reducing its permeability and destructive power.

 

The sample with 4% α-Al₂O₃ micropowder added (Sample c) shows good penetration resistance. As observed in Figure 3c, although its slag penetration layer is thicker than that of the conventional magnesia-carbon brick, its matrix is relatively dense. The in-situ formed spinel effectively preserves the integrity of the magnesia-carbon material and enhances its resistance to slag erosion.

 

For the sample with 6% α-Al₂O₃ micropowder added (Sample d, Figure 3d), the slag penetration layer is similar to that of the conventional magnesia-carbon brick. The matrix contains a certain amount of in-situ spinel bonding phase and corrosion-resistant periclase phase, giving the material both moderate penetration resistance and slag erosion resistance. At high temperatures, the introduced alumina reacts with magnesia to form magnesia-alumina spinel, and the resulting volume expansion reduces the pore size of the low-carbon magnesia-carbon brick, minimizing slag penetration depth.

 

XRD analysis of the sample with tabular alumina added (Sample e) confirms the presence of a spinel phase, and its porosity after sintering is close to that of the conventional magnesia-carbon brick (Table 2). However, due to the lower purity and larger particle size of tabular alumina compared to α-Al₂O₃ micropowder, the amount of magnesia-alumina spinel formed is insufficient to resist slag erosion at high temperatures, resulting in a greater slag erosion depth (Figure 3e).

 

As shown in Figure 3f (sample with 6% magnesia-alumina spinel added), although the periclase remains intact, slag has infiltrated the grain boundaries. This sample exhibits high porosity after sintering (Table 2), indicating that direct addition of spinel powder does not induce the micro-volume expansion effect associated with in-situ spinel formation. Consequently, the sintered sample has higher porosity, reduced resistance to slag erosion, and a greater erosion depth.

 

03 Conclusions

 

To investigate the effects of additives (α-Al₂O₃ micropowder, tabular alumina, and fused magnesia-alumina spinel) on the microstructure and slag erosion resistance of low-carbon magnesia-carbon bricks, the following conclusions are drawn:

 

At high temperatures, alumina reacts with magnesia to form spinel. The micro-volume expansion generated during spinel formation helps reduce the porosity of low-carbon magnesia-carbon bricks, refines the material's microstructure, and minimizes slag penetration and erosion.

 

In the low-carbon magnesia-carbon brick system, samples prepared with α-Al₂O₃ micropowder as the additive exhibit superior slag erosion resistance compared to those prepared with tabular alumina or pre-synthesized magnesia-alumina spinel powder.

 

When 4% α-Al₂O₃ micropowder is added, the volume expansion from in-situ spinel formation improves the compactness of the sample matrix, effectively preserves the integrity of the magnesia-carbon material, and enhances its resistance to slag erosion.