Formulation, Proportioning and Application Properties of Refractory Plastics
Refractory plastics are monolithic refractories composed of 70–80% granular and powdered materials, 10–25% binders such as plastic clay, and an appropriate amount of plasticizers. They have the consistency of a stiff paste and can maintain high plasticity over a long period.
Refractory plastics are mainly used in various heating furnaces that are not in direct contact with molten materials. Most are clay-based or high-alumina based; others include silica-based, magnesia-based, chrome-based, zircon-based, and silicon carbide-based types. According to the type of binder, they can be classified as clay-bonded, water-glass-bonded, phosphate-bonded, and sulfate-bonded plastics.
The aggregates used in refractory plastics mainly include super-grade calcined clay clinker and grade III, grade II, or grade I bauxite clinker. The maximum particle size of the refractory aggregate is 10 mm, with the following grading: 10–5 mm, 33%–40%; 5–3 mm, 28%–35%; below 3 mm, 28%–35%. It should be noted that particles in the range of 0.5–0.09 mm should be minimized or eliminated. The aggregate content is 55%–65%.
Refractory powders are generally made from super-grade, grade I, or grade II bauxite clinker. The fineness should be such that 95% passes below 0.09 mm; in practice, finer is preferable. Under-fired materials or clay clinker are strictly prohibited as refractory powder. The refractory powder content is 20%–30%.
To ensure ease of construction and reliable high-temperature performance, refractory plastics generally require the following basic properties:
① Sufficient plasticity for easy forming;
② A defined shelf life to maintain forming performance during the specified storage period;
③ Adequate strength after ambient curing to allow demolding or handling after installation;
④ Sufficient volume stability at high temperatures to prevent excessive deformation and damage to the furnace lining structure.
Since they are termed refractory plastics, what determines their plasticity?
The plasticity of refractory plastics is directly affected by the characteristics and dosage of clay and is also related to the water content. Plasticity increases with higher water addition; however, the water content should not be excessive and is generally controlled within 5–10%. To improve plasticity, both the clay content and water addition must be properly controlled, and external plasticizers may be used.
The functions of plasticizers in refractory plastics include:
① Improving the hygroscopicity of clay particles, dispersing fine clay particles, and forming a water film on their surfaces;
② Promoting the solation of clay particles;
③ Increasing electrostatic repulsion between clay particles to stabilize the sol;
④ Removing ions that hinder solation in the form of insoluble salts from the system;
⑤ Increasing the viscosity of water in the clay to form a strong water film.
Common plasticizers mainly include pulp waste liquor, naphthenic acid, lignosulfonate, lignin phosphate, and lignin chromate. The binders used in refractory plastics also affect plasticity to some extent.
Soft clay is a key raw material in refractory plastics, and the main performance characteristics of the plastics are derived from it. In refractory plastics, soft clay functions not only as a binder but also as a plasticizer and sintering agent. It significantly influences plasticity, water retention, workability, and both ambient and high-temperature refractory properties. Therefore, soft clay used in refractory plastics should have good plasticity, hygroscopicity, moderate adhesion, refractoriness, and sinterability.
In terms of forming and water retention, Guangxi clay and Fraxinus mandshurica clay exhibit the best viscoplasticity, while Fuzhou clay performs the worst. Jiaozuo clay can be used in combination with Zhangshu clay and Zimujie clay. The fineness should be greater than 85% passing below 0.09 mm, with a dosage of 10%–15%.
The chemical binder is an aluminum sulfate solution with a density of 1.2–1.3 g/cm³. After mixing with this binder, aging is required for no less than 16 hours. Aging is necessary because sulfate ions in aluminum sulfate react with iron in the powder to form ferric sulfate and release hydrogen, which can cause foaming or bulging of the mixture.
A pale yellow precipitate appears on the surface of the dried refractory plastic. Chemical and petrographic analyses identify it as iron alum with the formula FeO·Al₂O₃·4SO₃·22H₂O.
Figure 1 shows the differential thermal analysis (DTA) of aluminum sulfate and the surface precipitate on the plastic. It can be seen that most of the 18 molecules of crystal water in the aluminum sulfate solution are removed at approximately 134°C, with a small amount lost further at around 330°C. The endothermic peak above 835°C corresponds to the decomposition of aluminum sulfate into Al₂O₃ and gaseous SO₃, resulting in a slightly loosened microstructure and reduced strength of the refractory plastic.
The low-temperature endothermic peak on the iron alum DTA curve is due to the dehydration of crystal water. The endothermic peak at 752°C arises from the decomposition of iron alum and the release of SO₃, which also affects the strength of the plastic.

The extent of foaming in refractory plastics is directly related to the purity, density, and dosage of aluminum sulfate. In general, higher purity, higher density, and greater addition amounts result in increased foaming, which is caused by the larger amount of sulfuric acid introduced. Therefore, on the premise of meeting the requirements for plasticity, workability, and refractoriness, crude aluminum sulfate may be selected to prepare a low-density solution, and its dosage should be minimized as much as possible. The dosage of aluminum sulfate solution is generally 9%–13%.
Admixtures used in refractory plastics mainly include preservatives, plasticizers, reinforcing agents, and anti-corrosion agents. Other additives include sintering agents (also known as mineralizers), such as spodumene powder (LiO₂·Al₂O₃·4SiO₂), lepidolite powder (LiO₂·Al₂O₃·3SiO₂), and bentonite, as well as expansion agents such as kyanite or sillimanite.
There are many types of admixtures for refractory plastics. In addition to those listed in Table 1, polyvinyl alcohol, dextrin, starch, carboxymethyl cellulose, citric acid, gluconic acid, ethyl silicate, and others can also be used. The dosage of admixtures is generally less than 1%; when it exceeds 1%, they also function as binders. Other additives include andalusite, sillimanite, zircon, and alumina powder, with dosages generally greater than 3%.

Table 2 shows the mix proportions of aluminum sulfate-bonded refractory plastic. The maximum particle size of the refractory aggregate is 10 mm, the moisture content of the plastic is approximately 9%, and the plasticity index ranges from 17% to 30%.
In the table, "Sunan clay" refers to a composite of Suzhou clay and Nanjing clay: the former has a high sintering temperature, while the latter has a lower sintering temperature due to its higher content of low-melting components. "Super-grade clay clinker" and "Grade I bauxite clinker," etc., refer to super-grade calcined clay clinker and Grade I bauxite clinker, respectively. "Grade I + II bauxite" denotes a refractory powder prepared by mixing Grade I and Grade II bauxite clinker at a mass ratio of 1:1.
Admixtures are selected according to the service requirements of the refractory plastic, as shown in Table 1. For example, if the plastic is used immediately after production, preservatives and curing stabilizers may be omitted.