Glass Furnace Refractory Bricks: Key Parts, Operating Conditions & Matching Selection Guide

Aug 18, 2025

Leave a message

 

Refractory bricks in the main parts of the glass kiln use conditions and match selection

 

Refractories, as key components of glass kilns, have a decisive influence on glass quality, energy consumption, and production costs. The future development of glass melting technology depends, to a certain extent, on advancements in refractory manufacturing and improvements in product quality.

 

Furnace Construction for Glass Melting Kilns

 

For large float lines, the glass kiln is typically composed of several parts: an L-shaped hanging wall (usually made of silica bricks); a melting section (using electrofused bricks in areas in direct contact with molten glass, and silica or electrofused bricks for the crown area); a throat (commonly constructed with silica bricks); and a cooling section, including the doghouse (corundum is used for areas in direct contact with the molten glass, while silica or corundum is used for areas not in direct contact). Other components include the annealing lehr and the regenerator (constructed from high-alumina bricks, clay bricks, and directly bonded magnesia-chrome bricks).

 

Refractory Bricks for the Main Parts of the Kiln and Selection of Refractory Types

 

01. Crown (Swan Top)

 

The crown (also referred to as the swan top) of the melting and cooling sections of a glass melting kiln, including the arch, operates at a working temperature of around 1600°C. The refractory materials used in these areas must withstand high temperatures, mechanical loads, alkali vapors, and erosion from the batch materials. Therefore, the refractories used for the crown must have very high refractoriness, a high load softening temperature, good creep resistance, and low thermal conductivity. They must also be chemically stable at high temperatures and should not contaminate the molten glass. In addition, they should have low bulk density and high strength at elevated temperatures.

 

1.High-performance, high-purity silica bricks meet all of these requirements:

2.Their load softening point is close to their refractoriness.

3.They offer excellent stability at high temperatures and high compressive strength.

4.With SiO₂ content above 96%, their chemical composition is similar to that of glass, so under high temperatures, erosion by contact with molten glass does not lead to contamination.

5.They are cost-effective.

 

As a result, high-purity, high-quality silica bricks have become the preferred material for crown construction in various glass production processes.

 

Damage to crown bricks primarily results from chemical reactions at high temperatures between alkali vapors, dust, and the refractory material, as well as from crystalline transformations and structural densification caused by temperature fluctuations and physical phase migration. Research shows that deterioration of high-quality silica bricks used in glass kiln crowns is mainly due to the migration of impurities and heterogeneous phase transformations under high temperatures, while chemical corrosion and melting play a relatively minor role. Interestingly, the effects of phase transformation and self-purification can actually enhance the refractory properties of the bricks over time in the working zone, improving their high-temperature performance.

 

02. Pool Wall

 

1.Sections in Direct Contact with Molten Glass

 

In the melting and cooling sections, the areas of the pool wall in direct contact with molten glass are exposed to both chemical corrosion from the glass and physical erosion caused by its flow. The key requirement for refractory materials used in this area is excellent resistance to glass corrosion, while also ensuring that the refractories do not contaminate the molten glass.

 

In domestic glass kilns, it is common to use fused zirconia-corundum bricks, α-β corundum bricks, and β-corundum bricks for these applications.

Fused zirconia-corundum bricks perform exceptionally well at high temperatures and in resisting molten glass corrosion. These bricks form a eutectic of baddeleyite (ZrO₂) and α-Al₂O₃ during the electrofusion process, providing a high level of erosion resistance that cannot be achieved with sintered refractories. As a result, they are ideal for use as wall bricks in the melting zone of glass furnaces.

 

α-β corundum bricks and β-corundum bricks, whose main crystalline phase is corundum and which contain only 1–2% glass phase, also offer good corrosion resistance. However, compared to fused zirconia-corundum bricks, their lack of ZrO₂ crystals results in a reaction layer with lower viscosity and less thermal stability. This increases the diffusion rate between the refractory surface and the molten glass, leading to faster degradation of the kiln lining.

 

That said, at temperatures below 1350°C, α-β corundum and β-corundum bricks show better erosion resistance than fused zirconia-corundum bricks. Therefore, these bricks are more suitable for the cooling zone of the furnace, where operating temperatures are lower.

 

2.Sections Not in Direct Contact with Molten Glass

 

In the melting and cooling sections, the areas of the pool wall not in direct contact with the molten glass-often referred to as the breast wall-are primarily exposed to alkali vapor and batch dust erosion. Depending on design requirements, these areas may be constructed using either corundum materials or silica bricks, both of which can meet operational demands. In these locations, hooked or straight bricks are commonly used.

 

03. Regenerator (Checker Chamber)

 

1. Crown and Side Walls

 

The crown (roof) and side walls of the regenerator are subjected to high temperatures, dust, and alkali vapor corrosion. From top to bottom, the intensity of erosion gradually decreases. Therefore, the selection of refractory materials for the crown and side walls should be based on the operating temperature and degree of corrosion at different heights.

 

For the upper crown and upper side walls, silica bricks or high-quality silica bricks are generally recommended.

 

For the mid-section side walls, low-porosity clay bricks or high-alumina bricks are commonly used.

 

For the lower parts, ordinary clay bricks or low-porosity clay bricks are generally sufficient.

 

In recent years, depending on design variations, the upper side walls have also seen successful application of ordinary magnesia-chrome bricks, direct-bonded magnesia-chrome bricks, magnesia-alumina bricks, and other alkaline refractories.

 

2. Checker Bricks (Lattice Body)

 

Checker bricks are exposed to high temperatures, heavy loads, dust, and alkali vapors, and thus experience more severe erosion than the crown and side walls. Blockage or collapse of the checkerwork is a common reason for cold repairs during furnace shutdowns. Therefore, the checker bricks must meet the following requirements:

 

High physical strength,

 

Low creep rate,

 

Strong resistance to alkali corrosion, especially under fluctuating temperatures and atmospheres,

 

Low tendency for dust adhesion,

 

Slow and predictable wear over time.

 

Top of the Checkerwork

 

Temperature: 1400–1540°C

 

Conditions: Most severe alkali vapor and dust corrosion

 

Material: Electrofused re-bonded magnesia bricks are typically used. These bricks contain minimal silicate phase, feature large magnesia crystals, and have a direct bond structure that resists the increase in crystal size caused by alkali vapor attack-thereby preventing cracking and spalling.

 

Upper Section of the Checkerwork

 

Temperature: 1100–1430°C

 

Material: Generally uses 95# direct-bonded magnesia bricks.

 

Middle Section of the Checkerwork

 

Temperature: 800–1100°C

 

In this range, alkali metal sulfates condense, and magnesia and calcium-based refractories are seriously corroded by SO₃ and Na₂O, leading to excessive expansion and severe damage.

 

Material Recommendation: Magnesia bricks are not suitable here. Instead, use magnesia-alumina spinel bricks, direct-bonded magnesia-chrome bricks, magnesia-zirconia bricks, or magnesia-olivine bricks.

 

Lower Section of the Checkerwork

 

Temperature: Low

 

Although chemical attack is minimal, this section is close to the flue and exposed to cold air, causing rapid temperature fluctuations.

 

Material Requirement: Must withstand thermal shock.

 

Material: Generally, low-cost, low-porosity clay bricks are sufficient.