Fabrication and Installation of Regenerator and Small Furnace Steel Structures
① The positioning of the regenerator is based on the centerline of the melting furnace and the centerline of the small furnace. First, check and verify the elevation of the regenerator floor, the positioning dimensions of column pits, air exchanger foundations, etc., handed over by the civil construction unit. If there are errors or mistakes, rectify them in a timely manner. The positioning dimensions of the regenerator should be as accurate as possible, with measurement errors controlled within 1mm. After drawing ink lines on the floor, measure the error of each diagonal to check whether the regenerator and each chamber are square and free of deflection. At the same time, the elevation and relevant positioning dimensions should be temporarily marked in corresponding locations for random inspection and verification during installation and masonry. Before masonry of bricks, the number of brick layers and the height of relevant positions should be marked on the regenerator columns, or a brick count rod should be erected to control the masonry elevation and wall levelness of the regenerator. During the entire installation and masonry process of the regenerator, relevant dimensions should be inspected and verified at any time, and errors should be corrected or rectified promptly.
② For the fabrication of regenerator columns, depending on the design, regenerator columns are usually made of H-shaped steel, I-beam, or channel steel. All steel sections must be corrected to be straight, and the allowable deviation after correction should comply with the drawing requirements. For those not specified in the drawings, they should conform to the current national standard *Code for Construction Quality Acceptance of Steel Structure Engineering* (GB50205-2001). The bending of the regenerator column throughout its entire length should not exceed 8mm, the inclination of the flange plate should not exceed 3mm, the unevenness in the width direction of the flange plate should not exceed 1.5mm, the diagonal error at both ends of the column should not exceed 5mm, and the entire column should be straight without torsion, otherwise, it will directly affect the installation quality.
③ The small furnace bottom frame should be assembled and welded on the assembly platform, with the overall unevenness controlled within 1.5mm after welding. When channel steel is used for the small furnace bottom plate, the channel steel should be straight, non-twisted, and must be smooth and free of burrs. When steel plates are used as the small furnace bottom plate, the unevenness of the steel plate should be less than 1.5mm. Steel gratings can also be used as the small furnace bottom grid, with the unevenness controlled within 1.5mm.
④ For the installation of regenerator columns, first check whether the column pits meet the installation requirements, ensuring sufficient depth and accurate position. During installation, the columns should be accurately positioned and hoisted into place one by one, with no errors in position or direction. After the installation and adjustment of the columns are completed, they should be temporarily welded and fixed or fixed with adjustable temporary fixtures. Subsequently, install the connecting beams between the columns, which can also be installed during the wall masonry process. Upper palm irons and arch waste angles can be installed after the wall masonry is completed.
⑤ For the installation of small furnace steel structures, the small furnace bottom frame is installed after the melting section columns and regenerator columns are in place. It is crucial to note that **sufficient backward clearance must be left between the small furnace bottom frame and the regenerator columns**. During kiln drying, after the main arch of the melting section expands and the tie rods loosen, the melting section columns tilt outward, driving the small furnace to move backward. Therefore, graphite powder should be applied or roller bars should be placed between the small furnace bottom frame and the corbels on the regenerator columns. Stopper blocks should be welded at the support beams on the melting section columns to facilitate the overall backward sliding of the small furnace. The backward clearance between the small furnace bottom frame and the regenerator columns should be at least 50mm. If the small furnace cannot slide backward smoothly during kiln drying, it will pose serious quality hazards to the melting furnace.
⑥ Regenerator guard plates serve to prevent the wall from inclining inward and come in various structural forms. During installation, they should be flat and capable of sliding with the columns, not welded solid to avoid affecting the upward expansion of the wall. The regenerator arch waste angles should be fabricated straight, with an expansion joint of more than 20mm left between each section. When masonry arch waste bricks, they should be tightly attached to the arch waste angles, and any gaps must be packed tightly with steel plates, not with brick chips or refractory mortar.
⑦ The upper walkways, operation platforms, steel ladders, handrails, etc., of the regenerator are installed after the steel structure installation is completed, considering both operational convenience and the impact of steel structure thermal expansion.
Masonry of Refractory Materials for Regenerators and Small Furnaces
① The masonry works for regenerators, small furnaces, etc. shall be carried out in accordance with the current national standards such as the *Code for Construction and Acceptance of Industrial Furnace Masonry Engineering* (GB50211-2004) and the *Code for Construction and Acceptance of Float Glass Melting Furnace Masonry Engineering* (JCJ13), and constructed strictly in accordance with the design requirements.
② Refractory materials transported to the site shall be neatly placed by name, brick number, specification model, and masonry sequence. When handling refractory materials during transportation, they shall be lifted and placed gently to protect the integrity of the corners of refractory bricks. Refractory mortars must be stacked separately by different materials and shall not be damp or agglomerated. Mixers and mud containers shall be cleaned before use, and refractory mortars of different materials shall be mixed and used separately without confusion. The mortar for masonry bricks shall be compatible with the refractoriness and chemical composition of the bricks used.
③ During the masonry construction process, bricks shall not be chiseled on the masonry. When refractory bricks need to be processed, mechanical processing must be used. A wooden hammer or rubber hammer shall be used to align the bricks during masonry, and iron hammers are strictly prohibited. The masonry shall not be struck after the mortar has dried.
④ The regenerator walls must be masonryed straight and flat as per the design requirements, with brick joints no larger than 2mm, and built with staggered joints, full mortar, and the wall surface shall be cleaned without any remaining mortar. When masonrying bricks of different materials simultaneously, they shall be interlocked in layers as per the design requirements, with the principle that harder materials press on softer materials.
⑤ Expansion joints shall be set strictly in accordance with the design requirements. The expansion joints shall be masonryed straight and flat, kept clean inside, and free of mortar,dust and soil, and debris. The expansion joints in the wall shall be filled with polyethylene foam boards to prevent debris and dust from falling in and being difficult to clean. For expansion joints in contact with insulation bricks, the insulation bricks shall be replaced with hard bricks to cover the expansion joints. The wall shall not have expansion joints that are open inside and outside, and the joints shall be staggered by 230mm. As per the design requirements, vertical through expansion joints can be set, or upper and lower staggered expansion joints can be provided. The outer layer insulation bricks of the regenerator wall may or may not have expansion joints as per the design; generally, insulation bricks do not have expansion joints.
⑥ Arch bricks must be laid from both sides of the arch feet toward the center. If there is masonry behind the arch foot bricks, the arch shall only be laid after the masonry is completed. Before laying the arch, the arch bricks must be pre-arranged to determine the size of the brick joints. Inverting the large and small ends of arch bricks is strictly prohibited. The thickness of the locking brick (closure brick) shall not be less than 2/3 of the brick thickness. Do not directly strike the locking brick with a hammer to avoid damage or breakage; if a locking brick is damaged, it shall be replaced immediately. After the locking brick is driven in, the arch crown shall be grouted with thin mortar.
⑦ The arch formwork must be carefully fabricated according to the dimensions specified in the drawings. The arc and center shall be accurate, the structure stable, and the formwork surface must be flat without skew. After the arch is laid, the arch shall be tightened in a timely manner, and the formwork can only be removed after the arch is separated from the formwork and stabilized. The grid arch formwork must be removed before stacking the checkerwork to avoid damage to the grid arch from sudden heavy pressure.
⑧ The starting surface of the regenerator shall be leveled strictly according to the design elevation. The dimensions of the masonry wall shall be controlled as per the drawings. The wall shall be laid straight, and a brick layer elevation rod shall be set up to control the brick layer elevation. The flatness of the masonry shall be checked with a straightedge at any time, the verticality and levelness of the wall with a spirit level, the thickness of the brick joints with a feeler gauge, and the masonry dimensions with a steel tape measure. Any non-conformities with the masonry requirements shall be rectified promptly.
⑨ The laying of grid arches and leveling bricks is the key to regenerator masonry and shall be carefully constructed. Before laying, the quality of the grid bricks shall be inspected; any grid bricks with loose texture, cracks, bending, or twisting shall not be used, and the same applies to grid tie bricks. The grid arch formwork shall be supported flat and at the same height, and ink lines for each ring of grid bricks shall be marked on the formwork. Laying shall be carried out by pulling a line at the upper end, and the verticality of the grid bricks shall be checked with a spirit level during laying. The grid bricks shall be pre-arranged before laying to determine the thickness of the brick joints (no more than 2mm), laid simultaneously from both ends toward the middle, with each ring of grid bricks laid at the same speed. When reaching the position of the tie bricks, each ring of grid bricks shall be in a straight line. After checking with a straightedge and passing inspection, the tie bricks shall be laid; unqualified areas must be ground flat to ensure the tie bricks are not twisted or skewed. After laying the tie bricks, the grid bricks shall be pre-arranged again to determine that the thickness of the locking bricks is no more than 2/3 of the brick thickness, and every effort shall be made to avoid processing the locking bricks. The locking bricks shall not be too thin; if necessary, 2-3 grid bricks may be processed. The locking bricks shall be neither too tight nor too loose, generally about 50mm higher than the arch crown. After laying the locking bricks for each ring, the entire grid arch shall be finally adjusted to maintain verticality, uniform height, and overall straightness without twisting. Finally, the locking bricks shall be driven in simultaneously to ensure uniform stress on the entire grid arch. The purpose of laying leveling bricks is to ensure that the grid arches in each chamber of the regenerator are at the same level and height, laying a foundation for flat stacking of checker bricks. The levelness of each chamber must be controlled within ±1mm; non-conforming areas must be ground flat. The leveling bricks must be laid tightly against the grid arch, straight and flat. Leveling brick masonry for connected regenerators is more challenging and requires greater care.
⑩ During the masonry of the regenerator walls, the verticality and flatness of the masonry shall be frequently checked. The inner wall and the outer insulation wall shall be interlocked to avoid excessive cracking of the insulation layer during kiln drying. As the entire regenerator expands and rises significantly during kiln drying, at least 100mm of expansion space shall be reserved in the upper gap, and sufficient expansion gaps shall be left between the wall and the upper palm iron, between the wall and the arch waste angle steel, between the wall and the top steel plate, and between the partition wall and the regenerator arch. The regenerator walls use many types of bricks and mortars, which shall not be mixed during masonry. Acidic and alkaline bricks shall not come into direct contact and shall be effectively isolated. The electrofused corundum bricks at the small furnace opening shall be isolated from the wall with standard zircon bricks. Effective isolation shall be provided at the contact points between silica bricks and other bricks to avoid contact reactions at high temperatures that could affect the furnace life. After the regenerator wall masonry is completed, it shall be cleaned thoroughly, especially the inner side of the wall, which shall have no remaining mortar.
The checker bricks shall be laid flat according to the design requirements, with the upper surface horizontal and uniform spacing between checker bricks. If the upper surface is uneven, it shall be adjusted in a timely manner. The checkerwork shall be kept clean and unobstructed. In the actual operation of the melting furnace, collapse of the checkerwork occasionally occurs, especially in the later stage of operation. Apart from other factors, construction quality is also one of the causes. The construction method and precautions for the main arch of the regenerator are the same as those for the melting section. However, when tightening the main arch of the regenerator, the jackscrews behind the arch waste angle steel are tightened instead of the tie rods. Similarly, during kiln drying, the jackscrews are loosened instead of the tie rods in general cases.
Before masonry of the small furnace, it shall be checked whether the installation of the small furnace steel structure complies with the design requirements, and unqualified parts shall be rectified in a timely manner. Expansion joints and clearance gaps for the backward movement of the small furnace shall be reserved in the bottom bricks of the small furnace. Meanwhile, factors such as unevenness of the bottom plate caused by the upward expansion of the regenerator walls shall also be considered.
The side wall bricks, inclined arch bricks, and flat arch bricks of the small furnace shall be laid according to the pre-arranged numbering of the brick materials to avoid confusion. The side wall bricks and inclined arch bricks must be tightly attached to the breast wall of the melting section, and excessive brick joints are not allowed. The expansion joints between the small furnace and the regenerator must be masonryed as per the design requirements.
The masonry of the small furnace must take into account the following results caused by multiple factors:
Self-expansion of the brick materials used in the small furnace;
Overall backward movement of the small furnace during kiln drying;
Upward expansion of the regenerator walls;
Difficulty in operation during fire gap blocking;
Difficulty and intensity of furnace hot repair.
Therefore, every step must be carefully executed during furnace masonry, with attention paid to the operation of each detail, and every effort shall be made to eliminate any potential hazards.
Masonry of Face Bricks for the Melting Section and Cooling Section
① The laying of face bricks in the melting section and cooling section is carried out at the final stage of the furnace construction. After the face brick construction is completed, the interior of the furnace shall be cleaned, and finally, the furnace is sealed for kiln drying. The laying of face bricks must be strictly in accordance with the design requirements. Poor construction quality may cause material leakage at the bottom of the tank or bulging of face bricks after kiln drying, which is extremely difficult to handle, so meticulous construction is essential.
② According to the design requirements, there are multiple methods for constructing the face bricks (i.e., the tank bottom). A simple approach is to lay a 50mm layer of zircon corundum ramming material on large clay tank bottom bricks, followed by a 75-100mm layer of electrofused zircon corundum face bricks. Notes for this method: First, tape the joints of the large clay bricks to prevent the ramming material from entering the joints; second, the ramming material must be compacted thoroughly; and third, expansion joints in the face bricks must be set strictly according to the design. If construction is not meticulous, material leakage at the tank bottom may occasionally occur, especially around the temperature measuring holes in the tank bottom.
③ A currently more advanced method is to cast a layer of castable on the large clay bricks. The castable does not require expansion joints, providing a secure coverage of the entire tank bottom. After the castable solidifies, face bricks are masonryed with refractory mortar of the same material as the castable. The preparation, use, and construction method of the castable must strictly follow the design requirements. Non-shrinkage electrofused zircon corundum bricks are used for the face bricks, and expansion joints in the face bricks shall be set as per the design. It is important to note that the refractory mortar for masonrying face bricks must not enter the expansion joints, so it is recommended to use a suction cup for placing the face bricks during construction.
④ After the face brick construction is completed, tape the expansion joints and finally cover them with colored strip cloth to keep them clean. The laying of joint cover bricks must also leave sufficient expansion joints as per the design requirements.
Cleaning Inside the Furnace
In order to ensure the production of high-quality glass products as soon as possible, a thorough cleaning of the furnace interior must be carried out after the entire melting furnace construction is completed. Excess mortar and debris should be swept away, the covering colored strip cloth should be removed, and the gaps of the melting furnace should be sealed. A final inspection should be conducted on the flue, regenerator, melting section, cooling section, small furnace, throat, pendant wall, etc. After everything is confirmed to be correct, the melting furnace should be sealed.
There are many factors affecting the service life of a float glass melting furnace, including whether the furnace structure design is reasonable, whether the selected steel and refractory materials are appropriate, whether the quality of the materials used in the furnace is qualified, the management level of the furnace-using enterprise, and the operation and maintenance level of the actual furnace operators. It is undeniable that the construction quality of the melting furnace is also a very important factor. Therefore, it is particularly necessary and important to improve the construction quality of float glass melting furnace projects. Among them, enhancing the management level of the furnace construction unit and the management and technical level of the construction unit will both play a positive role in improving the construction quality of the melting furnace.
Masonry Technology of Unit Kiln Furnace
Masonry quality has a significant impact on the service life of kilns, fuel consumption, glass melting, and wire drawing operations. To meet the basic requirements of kilns for brick masonry dimensions and thermal expansion of the kiln body, the pool wall bricks and pool bottom facing bricks of the kiln must be cut and ground. Additionally, the reasonable reservation of expansion joints between kiln refractory bricks is also an extremely important link.
(1) Steel Frame Acceptance and Pre-Masonry
① According to the kiln construction benchmark line and the kiln centerline, steel structure layout construction is carried out. The main and secondary beams and flat steel are laid according to the steel structure design requirements and construction allowable deviations, while the steel structure of the channel is also constructed.
② To ensure masonry construction quality and progress, pool wall bricks, pool bottom facing bricks, and all load-bearing arch bricks with strict requirements for dimensions and brick joints shall undergo pre-masonry. However, if the dimensional accuracy of the above bricks is extremely high and fully complies with design requirements, pre-masonry may be omitted. All bricks subjected to pre-masonry must be numbered in sequence and installed in corresponding positions during formal masonry.
(2) Masonry Sequence and Methods
① Based on the acceptance of the pool bottom steel structure, the centerlines of the charging port, front and rear rows of bubbling points, and each wire drawing bushing on the forming channel are laid out according to the kiln construction benchmark line and the kiln centerline.
② Pool bottom masonry, including the channel bottom. After laying insulation bricks and large kaolin bricks, level the inside and outside of the pool wall masonry area with a width of 30-50mm. For multi-layer pool bottom structures, the construction must be controlled by negative elevation deviations, and the allowable deviation for the total thickness of the pool bottom is generally -3mm. A layer of zircon ramming material is laid on the large kaolin bricks of the pool bottom as a sealing layer to prevent glass liquid from penetrating into the clay brick layer with poor corrosion resistance.
③ Pool wall masonry, including channel pool walls. The bottom bricks of the pool wall must ensure levelness; otherwise, the bottom bricks at that part must be processed until the requirements are met. When masonry multi-layer pool wall bricks, operate from the inside to the outside to ensure the internal dimensions of the furnace, and it is strictly prohibited to face the chiseled surface of the bricks toward the furnace. The corners of the wall must be masonryed with staggered joints to strictly maintain verticality.
④ Hoist and install columns. Use temporary measures to stabilize the columns, then install arch waste angle steel according to design requirements. The columns and arch waste angle steel must be closely attached, and the elevation must be accurately determined.
⑤ Masonry the main arch. After manufacturing the arch formwork and conducting a load settlement test and corresponding dimensional inspection on the arch frame, the main arch is masonryed simultaneously from both sides toward the center, requiring continuous operation and completion within 24 hours as much as possible. The thermal insulation layer construction of the main arch is carried out after the kiln drying is completed.
⑥ Masonry the breast wall, front wall, rear wall, and channel flame space. The masonry of the breast wall shall be carried out after carefully inspecting the qualified installation of brackets, support plates, and support frames. Measures must be taken to prevent the hook bricks and breast wall bricks from falling into the kiln.
⑦ Masonry flues and chimneys. Masonry must be carried out after removing debris inside the kiln and vacuuming it clean. The masonry of the melting furnace flue and chimney shall also coordinate with metal heat exchangers, and the channel chimney must be masonryed after the channel masonry is completed.
⑧ There are two masonry methods: dry masonry and wet masonry.
a. Dry masonry parts: Pool bottom and walls of the melting section and channel, hook bricks in the flame space, arch waste bricks in the melting section and flue, electrofused brick masonry, and channel top cover bricks.
b. Wet masonry parts: Side walls and arch crowns of the flame space in the melting section, flues, chimneys, and thermal insulation bricks of the kiln. The mortar used for wet masonry shall be prepared with corresponding refractory mortar according to the refractory bricks used.
(3) Masonry Quality Requirements and Inspection
① Brick Joint Requirements: The gaps between bricks should be small. The allowable thickness of brick joints in masonry at various parts of the space generally does not exceed 2mm. The brick joints of the arch crown are required to be less than 1mm, and those of insulation bricks can be expanded to 3mm.
② Expansion Joints: Refractory bricks expand when heated, and expansion joints shall be reserved according to the type of brick and the temperature conditions of the location. The average value of expansion joints reserved in every 1m length of masonry can be calculated using the average linear expansion coefficient α. The expansion joints for pool bottom and wall bricks should be appropriately reduced to prevent insufficient expansion. The average expansion joints for dense chrome bricks and dense zircon bricks, the main refractory materials used in glass unit kilns, are approximately 5mm. Expansion joints shall be evenly segmented (with a spacing of no more than 2m), reserved in a closed manner between inner and outer brick layers, staggered between upper and lower brick layers, kept clean inside the expansion joints, and the outer layers shall be sealed with tape.
③ Allowable Errors: Strict allowable error ranges are specified for elevation, levelness, verticality, linear dimensions, and the flatness of the masonry surface. The brick joints of the masonry are inspected with a feeler gauge, and the thickness of the feeler gauge shall be equal to the specified thickness of the brick joints being inspected. The flatness is inspected with a 2m straightedge in all directions. After all inspections are completed and the kiln interior is cleaned multiple times, sealing treatment is carried out to minimize the re-entry of external debris and dust into the kiln body.