How To Solve Severe Ring Formation in Rotary Kilns While Normal Kiln Skin Hanging?

Oct 09, 2025

Leave a message

 

How to Solve Severe Ring Formation in Rotary Kilns While Normal Kiln Skin Hanging?

 

 Rotary Kiln Ringing

 

A rotary kiln ring refers to the phenomenon of a ring-shaped adhesion on the inner wall of the rotary kiln in the high-temperature zone. The slight adhesion is known as "kiln skin." However, when significant adhesion occurs, it can affect the normal operation of the kiln, which is referred to as "ringing."

 

 The Hazards of Ringing

 

The "ring" in a rotary kiln typically forms at a certain distance from the kiln's entrance, near the combustion points where solid fuel is concentrated. It occurs close to the refractory kiln lining, with a thickness ranging from 200 to 500 mm. The following are the main hazards of the "ring" in rotary kiln production:

 

1) Reduced Production and Increased Labor Intensity

 

Once the kiln ring forms, it inevitably obstructs the hot airflow generated by fuel combustion, as shown in Figure 1. The hot airflow is partially blocked in the A zone, which affects the effectiveness of lime roasting. At the same time, since the drying and preheating process in the preheater uses the kiln exhaust gas, the ring also negatively impacts the drying and preheating of lime. Specifically, the permeability is poor, the flame cannot reach the area, the rear temperature is low, moisture in the lime is difficult to remove, and lime cracking and pulverization become more severe. This leads to lower yields and reduced labor productivity.

 

In addition, once the ring forms, if not dealt with in time, its longitudinal length and thickness will increase. When the ring eventually falls off, it will increase the labor intensity of workers. In some cases, the kiln may need to be stopped for maintenance, which further affects the kiln's output.

 

2) Increased Equipment Load

 

As shown in Figure 1, the formation of a knot ring with a certain area and thickness causes the material flow to be blocked in the B zone. At this point, the amount of blocked material is much higher than normal. Combined with the weight of the ring itself, this inevitably increases the wear and tear on the wheels and bearings. Additionally, it increases the load on the motor, which can even lead to motor failure or burning.

1

3) Waste of Energy

 

In actual fire-watch operations, when a "ring" forms, the hot gas flow is blocked in the A zone. To ensure proper drying in the preheater and maintain the preheating effect, fire-watch workers tend to increase the amount of coal fed into the system. This, however, inevitably leads to a waste of energy.

 

 Causes of Ringing

 

The cause of ringing in production can be summarized as improper operation. Specifically, it occurs due to an excessively large quantity of feed, poor drying effects, and the bursting of raw materials. This leads to severe pulverization, resulting in poor permeability. As a result, the induced draft fan has difficulty drawing the flame, and the flame is only able to burn at a certain distance from the kiln. At temperatures greater than 1200°C, a portion of the SiO₂ in the limestone, which has not fully oxidized, reacts to form a liquid phase.

 

Additionally, when the coal feed is excessive, and under the condition of 1150°C, the interaction between CaO and SiO₂ generates CaO-SiO₂, forming a slag phase that binds the materials. As the materials flow through the roasting zone, the resulting liquid and slag phases are very likely to adhere to the kiln lining. This causes the bonding of materials, leading to the formation of the ring phenomenon.

 

①The Composition of Raw Materials and Kiln Operation Fluctuations

 

The composition of raw materials entering the kiln fluctuates significantly, and the feeding quantity is unstable. As a result, kiln materials can sometimes be difficult to burn and, at other times, burn well. This fluctuation is one of the kiln operator's biggest challenges. When encountering high KH materials, the kiln material becomes loose and difficult to sinter, which causes the kiln head to "eat fire." The clinker may have high fCaO content. In such cases, operators are forced to add more coal to increase the firing temperature and, at times, reduce the kiln speed. On the other hand, when dealing with low KH materials or insufficient quantities, kiln operation may not be adjusted in time, leading to a high firing zone. This results in overcooking of the material, making it more viscous, and, with the slightest oversight, long, thick raw material can form, eventually leading to the creation of kiln skin. This, in turn, can result in the formation of clinker rings.

 

② Influence of Harmful Components

 

An analysis of the ring material shows that the content of CaO, Al₂O₃, Fe₂O₃, and SiO₂ is low, while the content of R₂O and SO₃ is high. The harmful components in the raw material undergo successive decomposition, gasification, and volatilization during the clinker calcination process. These components then cohere and adhere to the surface of the raw material particles at the lower temperature end of the kiln. As the raw materials move with the kiln, it is easy for a sulfur-alkali ring to form at the back end of the kiln.

 

In the raw material, when the magnesium oxide and R₂O content is high, R₂O acts as a medium to form a magnesium-alkali ring during the process of magnesium oxide-induced ring formation. According to the practical experience of cement manufacturers, when the magnesium oxide content in clinker exceeds 4.8%, it significantly increases the amount of liquid phase in the clinker. This results in a decrease in the viscosity of the liquid phase, narrowing the sintering range of the clinker, promoting the growth of kiln skin, and causing the floating kiln skin to thicken. Some cement manufacturers report that even when the magnesium oxide content in clinker is less than 4.0%, the fluxing effect of R₂O can still lead to a substantial increase in the liquid phase at certain temperatures or specific locations within the kiln. This drastically reduces the viscosity of the liquid phase, causing the material to bond at certain regions, resulting in the formation of clinker rings.

 

③Influence of Pulverized Coal Quality

 

High ash content, coarse fineness, high moisture, and high ignition temperature in pulverized coal lead to slow combustion, a long black fire head, and an increased likelihood of incomplete combustion. The concentrated ash settlement can also cause clinker rings to form. In addition to unstable coal feed amounts, high or low kiln temperatures can further promote the formation of these rings.

 

④Influence of Primary Air Volume and Secondary Air Temperature

 

With a three-channel or four-channel burner, a large primary air volume and high secondary air temperature can cause the coal dust exiting the nozzle to ignite. This results in high combustion temperatures, concentrated flames, a shorter firing zone, and a position near the front of the kiln, all of which make the formation of a kiln ring more likely. This phenomenon is often referred to as the "front ring."

 

 Handling Method

 

To reduce or eliminate the ring phenomenon, the first step in production is to take preventive measures. This involves using correct operating procedures, maintaining a stable feeding volume, and ensuring that the material layer thickness is appropriate. This will help guarantee proper drying and preheating effects, reduce the bursting and pulverization of lime, and control the amount of coal fed into the kiln. The coal feed should not be excessive, as this can keep the temperature within a lower range and prevent the formation of the slag phase.

 

If a ring forms, it must be dealt with promptly. Otherwise, it may lead to the adverse consequences of the kiln wall widening and thickening, which increases the difficulty of handling and can even disrupt normal production.

 

There are three methods for removing rings, as follows:

 

(1)Installing a moving alloy scraper in the kiln;

(2)Adding an appropriate amount of fuel to sinter the bond; and

(3)Adjusting the high-temperature zone.

 

Comparatively speaking, the first method, using a scraper, requires specific materials that are difficult to achieve. The second method is feasible, but from an energy-saving perspective, it is not ideal and is also challenging. The third method, however, is considered a feasible approach based on practical experience.

 

The so-called "appropriate change" in the high-temperature zone involves adjusting the opening and closing of the rear induced draft fan's fan box flap. This allows the combustion point or flame to move back and forth, making it easier for the bonded kiln ring to fall off, thus achieving the goal of eliminating the ring. This method not only saves energy but is also simple and easy to operate.