Magnesia-Chromite Refractories Degradation Mechanism in Copper Smelting Side Blowing Furnaces

Mar 26, 2026

Leave a message

 

Magnesia-Chromite Refractories Degradation Mechanism in Copper Smelting Side Blowing Furnaces

 

Side Blowing Furnace

 

Side-blowing furnaces are widely used in the smelting and processing of non-ferrous metals such as gold, silver, copper, lead, and tin. Refractory materials for the lining of side-blowing furnaces must have high temperature resistance, good thermal stability, high refractoriness under load, excellent oxidation resistance, outstanding resistance to high-temperature molten metal and melt erosion, as well as non-reactivity with smelting slag.

 

Given the above performance requirements for lining materials in side-blowing furnaces, magnesia refractories are commonly used as the inner lining. To improve the corrosion resistance of the lining, areas in contact with copper matte melt and slag - such as the furnace hearth and slag chamber - are mostly lined with magnesia-chromite refractories containing a high content of Cr₂O₃.

 

In recent years, research on copper smelting furnace technologies and refractory degradation mechanisms, both domestically and internationally, has mainly focused on furnace types including the Ausmelt furnace, Isasmelt furnace, bottom-blowing furnace, and converter. Relatively few studies have been conducted on the degradation mechanisms of magnesia-chromite refractories in side-blowing furnaces.

 

To ensure the safe and stable operation of side-blowing furnaces under new processes and to extend the service life of lining materials, this study analyzes the corrosion and damage mechanisms of used magnesia-chromite bricks from harsh-service zones of existing side-blowing furnaces. It is expected that the findings will provide a reference for improving the quality and innovating magnesia-chromite refractories used in side-blowing furnaces.

 

Experiments

 

1.1 Sample Preparation

 

An analysis was conducted on the corrosion behavior and mechanisms of spent magnesia-chromite bricks that had been in service for 20 months in the side wall at the slag line of a side-blowing furnace in a copper smelter. Spent brick No. 6 at the slag line and spent brick No. 8 above the slag line were selected as test samples. Specimens with dimensions of 40 mm × 20 mm × 5 mm were cut using a small diamond cutting machine. After curing with epoxy resin at 50 °C for 3 hours, the specimens were ground and polished using an automatic pressure grinding and polishing machine to prepare samples containing the slag adhesion layer, the altered layer (a dense layer below the slag zone with significantly different macro-morphology from the original brick), and the original-like brick layer (a zone with minor differences in macro-morphology from the original brick).

 

1.2 Testing and Characterization

 

The contents of SiO₂, Al₂O₃, Fe₂O₃, and K₂O in the post-service smelting slag were determined according to GB/T 6730.10-2014, GB/T 6730.11-2007, GB/T 6730.65-2009, and GB/T 6730.49-2017, respectively. The contents of minor components were tested in accordance with GB/T 34333-2017. Microstructure and micro-area composition analysis of the spent magnesia-chromite brick samples were performed using a ZEISS EVO-18 scanning electron microscope equipped with an energy-dispersive X-ray spectrometer.

 

Results and Discussion

 

2.1 Pre-service Magnesia-Chromite Brick

 

The apparent porosity and bulk density of the fused rebonded magnesia-chromite brick were 13.4% and 3.35 g·cm⁻³, respectively. Its chemical composition (mass fraction) was as follows: MgO 55.42%, Cr₂O₃ 22.88%, Fe₂O₃ 12.29%, Al₂O₃ 6.34%, SiO₂ 0.74%, CaO 0.76%. The morphological characteristics of the original brick are shown in Figure 1. Figure 1(a) presents the bonding characteristics between aggregates and the matrix of the magnesia-chromite brick, showing tight bonding between aggregates and matrix. Figure 1(b) shows the phase distribution in the matrix, indicating that the matrix mainly consists of chromite, periclase, and spinel phases precipitated within and between periclase crystals. In addition, a small amount of forsterite phase (M₂S) was also precipitated between periclase grains.

 

01

 

2.2 Test Slag

 

The chemical composition (mass fraction) of the slag discharged from the smelting process in the side-blowing furnace is as follows: SiO₂ 27.05%, Al₂O₃ 4.90%, Fe₂O₃ 60.20%, CaO 2.20%, ZnO 1.99%, MgO 1.54%, CuO 1.10%, K₂O 1.02%.(In this work, all iron content from chemical analysis is expressed as Fe₂O₃, whereas iron in ferrosilicon slag under smelting conditions mostly exists in the form of FeO.)

The mass ratio of Fe to SiO₂ is 1.53, and the mass ratio of CaO to SiO₂ is 0.08.

The refractoriness of the slag was measured to be 1380 °C, its softening temperature is 1450 °C, and its flow temperature is 1470 °C.

 

2.3 Macro-morphology of Spent Magnesia-Chromite Bricks

 

A schematic diagram of the structural changes in the side wall at the slag line after service is shown in Figure 2.

Spent magnesia-chromite bricks No. 4 and No. 5 are located below the slag line, with no obvious slag adhesion on their surfaces.

In contrast, spent bricks No. 7 and No. 8 are situated above the slag line and have a relatively thick slag adhesion layer.

Brick No. 6 is located at the slag line, at the interface between molten slag and copper liquid; a distinct slag adhesion layer can be observed above the slag line, while no obvious slag adhesion exists below it.

The residual thicknesses of the spent magnesia-chromite bricks and the thicknesses of the slag adhesion layers on their surfaces are listed in Table 1.

The residual thicknesses of bricks No. 7 and No. 8 above the slag line are greater than those of bricks No. 4 to No. 6.

Moreover, the thickness of the slag adhesion layer on bricks above the slag line tends to increase with increasing distance from the slag line.

Brick No. 6 at the slag line exhibits the smallest residual thickness.

The region above the slag line is mostly in contact with molten slag, allowing a protective slag adhesion layer to form on the magnesia-chromite brick surface, resulting in a lower erosion rate than that of bricks below the slag line, which are in contact with copper liquid.

Since brick No. 6 is located at the slag line, it is subjected to alternating scouring, penetration, and corrosion by both copper liquid and molten slag, leading to the highest erosion rate.

 

02

1

 

Figure 3 shows cross-sectional photographs of spent magnesia-chromite bricks No. 6 and No. 8 after service.

By comparing bricks No. 6 and No. 8, the thickness of the dense altered layer on their hot faces is approximately 1 mm for both.

 

It is inferred that, under such service conditions, frequent temperature fluctuations result in continuous thickness loss on the hot face of the magnesia-chromite brick due to scouring and thermal stress spalling, without forming a thick, distinct, and continuous dense altered layer beneath the hot face.

 

However, most studies on the corrosion and degradation analysis of magnesia-chromite bricks used in copper smelting furnaces have reported the formation of a relatively thick altered zone with obvious stress cracks within it.

This indicates that the degradation mechanism of magnesia-chromite bricks at the slag line of this side-blowing furnace is significantly different from that of magnesia-chromite bricks under the furnace types and service conditions mentioned in the literature.

 

03

 

2.4 Damage Analysis of Spent Magnesia-Chromite Bricks

 

2.4.1 Spent Magnesia-Chromite Brick No. 6 Below the Slag Line

 

A comparative analysis of the microstructure and EDS composition of brick No. 6, both above and below the slag line, revealed that although there was a significant difference in slag adhesion between the upper and lower parts, the microstructure, phase composition, and EDS elemental composition of the altered layer and the original-like brick layer were similar in both regions.

 

Therefore, the corrosion mechanism was analyzed only based on the microstructure, chemical composition, and phase composition of brick No. 6 below the slag line; the part above the slag line was not described again.

Figure 4 shows the microstructure photographs of the hot face of spent brick No. 6.

 

04

 

It can be seen from Figure 4 that, from top to bottom at the hot face, there are successively the slag layer, the reaction layer (where the molten slag reacts with the original brick, resulting in significant changes in the composition and morphology of the matrix and aggregates), and the penetration layer (where the molten slag penetrates along pores and grain boundaries without obvious corrosion reactions, and the composition and morphology of the matrix and aggregates remain basically unchanged).

In the slag layer, the main phases are spinel and an olivine-like phase [MFS: (Mg,Fe)₂SiO₄].

In the reaction layer, the periclase and chromite in the original brick matrix are clearly dissolved and separated, forming a large amount of spinel and a small amount of olivine phases, accompanied by the penetration of Cu₂S and FeS; the thickness of the reaction layer is approximately 1 mm.

In the penetration layer, the periclase and chromite grains of the magnesia clinker remain intact, and the slag corrosion reaction is significantly weakened.

 

Figure 5 shows the microstructure photograph of the reaction layer in Figure 4. EDS analysis was carried out on its typical phases, and the results are listed in Table 2.

Analysis of its chemical composition shows that the main phases are Cu₂S, FeS, Al-Fe-Cr spinel, Mg-Fe olivine, and Mg-Al-Fe-Cr spinel.

That is to say, at the hot face of spent magnesia-chromite brick No. 6, the periclase phase in the original magnesia-chromite brick reacts with SiO₂ and FeO in the ferrosilicon slag to form low-melting Mg-Fe olivine. Meanwhile, the magnesia-chromite clinker and chromite dissolve and absorb Al₂O₃, FeO, and other components from the ferrosilicon slag, forming Fe-Al-Cr spinel and Mg-Fe-Al-Cr spinel.

 

05

 

Figure 6 shows microstructural photographs of spent brick No. 6 at different distances from the hot face.

It can be observed that a large amount of copper matte (bright white regions) is distributed throughout, extending from the hot face up to 35 mm away from it.

At positions 1–35 mm from the hot face, matrix pores and grain boundaries are infiltrated and filled with a large amount of copper matte, which wraps around magnesia and chromite grains.

This destroys the bonding between magnesia-chromite clinker, chromite, and periclase, and damages the structural stability of the magnesia-chromite brick.

 

06

07

 

According to EDS analysis, copper exists in the matrix of the magnesia-chromite brick only in the form of Cu₂S.

Table 3 shows a comparison of the chemical composition of copper matte in the slag layer of spent brick No. 6 and at distances of 1 mm and 20 mm from the hot face.

It can be seen that the proportions of Cu, Fe, and S in the copper matte at 1 mm and 20 mm remain basically unchanged, indicating that only the penetration of copper matte occurred in the magnesia-chromite brick during the smelting process, without obvious corrosion reactions with the matrix and grains of the brick.

 

Compared with the slag layer, the copper content at 1 mm and 20 mm is higher, while the iron content is lower.

This demonstrates that the penetration ability of Cu₂S in copper matte is stronger than that of FeS in the magnesia-chromite brick.

 

2

 

Table 4 shows the EDS analysis results of the slag layer of spent brick No. 6 and at various distances downward from the hot face.

It can be observed that:

 

1)The contents of SiO₂ and CaO at distances of 1–35 mm from the hot face are similar, indicating that during copper smelting, the penetration of SiO₂ from the molten slag and its reaction with the magnesia-chromite brick occurred only at the hot face and did not further penetrate into the interior of the brick;

 

2)Compared with the chemical composition of the original brick, the contents of CuO and SO₃ at 1–35 mm are significantly increased, which further confirms the deep inward penetration of copper matte in the magnesia-chromite brick.

 

3

 

Figure 7 shows the penetration path of copper matte in spent brick No. 6.

It can be seen that copper matte mostly penetrates around chromite grains and along grain boundaries of secondary precipitated iron-rich spinel.

This phenomenon is related to the small wetting angle between the iron-rich chromite/secondary crystallized iron-rich spinel phases and copper matte, which favors the penetration of copper matte into the magnesia-chromite brick.

 

Therefore, high-purity magnesia clinker, high-purity fused magnesia-chromite clinker, and low-iron chromite are recommended to suppress the precipitation of iron-rich phases during the firing of magnesia-chromite bricks, improve the bonding strength of the bricks, and reduce the penetration of copper matte.

Literature indicates that under the same process conditions, improving the grade of magnesia and magnesia-chromite clinker can enhance the properties of magnesia-chromite refractories, thereby improving their corrosion resistance and penetration resistance.

 

08

 

Based on the above microstructure and EDS analysis of spent magnesia-chromite brick No. 6, the following mechanisms can be concluded at the slag line:

 

1)SiO₂ and CaO in the ferrosilicon slag react with MgO dissolved from periclase at the hot face to form low-melting silicate phases. The penetration and corrosion of SiO₂ and CaO into the magnesia-chromite brick can proceed only after the hot face has been eroded and spalled;

 

2)Meanwhile, copper matte penetrates along pores and grain boundaries, and the penetration ability of Cu₂S in copper matte is stronger than that of FeS;

 

3)Although copper matte does not participate in the corrosion reaction with the magnesia-chromite brick, it wraps around magnesia-chromite clinker, chromite, and magnesia grains, weakening the bonding of the brick. This reduces the resistance of the magnesia-chromite brick to penetration and corrosion by other high-temperature melts, thus accelerating its degradation.

 

2.4.2 Spent Magnesia-Chromite Brick Above the Slag Line

 

Figure 8 shows the microstructure photograph at the hot face of spent brick No. 8 above the slag line. Combined with the EDS elemental mapping in Figure 9, it can be seen that, unlike brick No. 6, brick No. 8 forms large-sized fayalite (F₂S, approximately 200 μm) at the hot face.

Beneath the fayalite lies a dense iron-rich spinel layer (Fe₂O₃ mass fraction = 89.8%), and below the spinel layer is a dense magnesio-ferrous olivine (MFS) layer.

This indicates that the hot face of the magnesia-chromite brick above the slag line is exposed to relatively stable molten slag, providing favorable thermal and dynamic conditions for the reaction between the slag and the brick to form dense layers of olivine and secondary spinel.

The dense spinel layer and magnesio-ferrous olivine layer effectively prevent further penetration and corrosion by molten slag and copper matte, slow down changes in the structure and composition of the magnesia-chromite brick, and reduce its structural spalling rate.

 

09

10

 

Figure 10 shows microstructural photographs of spent brick No. 8 at different distances from the hot face.

As can be seen from Figure 10, compared with the microstructure of spent brick No. 6:

 

1)Although brick No. 8 is located above the slag line, copper matte still penetrates into it, but the penetration depth is significantly reduced.

With increasing distance from the hot face, the number of pores not filled by copper matte gradually increases.

Table 5 shows the EDS analysis results of brick No. 8 at different distances from the hot face.

Compared with the copper matte content in brick No. 6 at the same distances from the hot face, the content in brick No. 8 is noticeably lower.

 

2)The degree of reaction between molten slag and the magnesia-chromite brick in the reaction layer of brick No. 8 is weaker than that in brick No. 6.

In brick No. 8, parts of the reaction layer and chromite grains only undergo decomposition and secondary spinel formation at the grain edges, and the grain boundaries remain relatively distinct.

 

11

4

 

In summary, magnesia-chromite brick No. 8 was subjected to both copper matte penetration and simultaneous penetration and corrosion by SiO₂-FeO slag. However, the amount of copper matte that penetrated into brick No. 8 was less than that in brick No. 6. Moreover, a dense and continuous layer composed of spinel and magnesio-ferrous olivine formed on the hot face of brick No. 8, which, to some extent, prevented further penetration of copper matte and further penetration and corrosion by SiO₂-FeO slag. This helped reduce structural damage to the brick caused by SiO₂-FeO slag and copper matte and lowered the erosion and spalling rate of the magnesia-chromite brick.

 

Conclusions

 

(1)The erosion rate of magnesia-chromite brick at the slag line was higher than that of the brick above the slag line. At the slag line, the brick was exposed to repeated scouring, penetration, and corrosion by the copper matte melt and SiO₂-FeO slag. As a result, a stable protective slag layer could not form, leading to the highest erosion rate.

 

(2)An approximately 1-mm-thick altered layer beneath the hot face was observed in cross-sections of spent magnesia-chromite bricks both at and above the slag line. It is inferred that the altered layer formed by slag penetration and corrosion could not remain stable on the hot face during service. The brick underwent penetration and corrosion reactions with copper matte melt and SiO₂-FeO slag, followed by hot face spalling. Therefore, the service life of magnesia-chromite bricks can be improved by increasing the density and bonding strength of magnesia-chromite materials, enhancing their penetration and corrosion resistance, reducing the thickness of the altered layer, or stabilizing the smelting process and reducing temperature fluctuations to minimize thermal spalling.

 

(3)Copper matte penetration and SiO₂-FeO slag corrosion occurred in spent magnesia-chromite bricks both below and above the slag line. In both cases, reactions between SiO₂-FeO slag and the bricks formed low-melting olivine phases and secondary spinel phases. However, internal copper matte penetration was much more severe in bricks at the slag line. After penetration, copper matte wrapped around matrix grains such as chromite, destroying the bonding strength of the brick and significantly reducing its thermal shock resistance and spalling resistance against copper matte melt and SiO₂-FeO slag. Above the slag line, copper matte penetration was weakened, and corrosion by SiO₂-FeO slag became the dominant hot-face reaction. A dense secondary spinel layer and magnesio-ferrous olivine layer formed on the hot face, which reduced penetration of molten slag and copper matte melt into the brick, lessened structural damage, and slowed the erosion rate.

 

(4)Copper matte mainly penetrated along grain boundaries and pores around chromite grains, as well as between periclase crystals where iron-rich spinel precipitated. This was detrimental to the penetration and corrosion resistance of magnesia-chromite bricks against SiO₂-FeO slag. The penetration depth of copper matte into the brick can be reduced by improving raw material purity, lowering FeO content in chromite and magnesia-chromite clinker, and suppressing precipitation of Fe-containing phases, thereby reducing the erosion rate of magnesia-chromite bricks.