Performance and Application Comparison of Conventional and High-Performance Magnesia-Chrome Bricks
The flue of a metallurgical furnace in a steel plant was changed from bidirectional flow to unidirectional flow, resulting in a 300–500°C increase in the flue gas temperature inside the exhaust system, including the riser wall, supporting arch, transition zone, vertical flue roof, and other components mentioned in this paper. This has severely affected the operation of the downstream system.
Using water spray to reduce the flue gas temperature caused serious hydration damage to the brick lining in the exhaust system. Moreover, large temperature fluctuations during the smelting and tapping periods led to severe cracking and spalling of the brick lining, and even to accidents such as roof collapse and wall failure.
Therefore, research, development, and practical application of lining bricks for the flue have been carried out. The details are presented as follows.
Trial Analysis
The properties of the trial formulations of ordinary magnesia–alumina bricks and the developed magnesia–chrome bricks are listed in Table 1. The condition of the residual bricks after 1–2 furnace campaigns is shown in Figure 1.


The typical properties of magnesia–chrome bricks produced by a special process based on Formula A, together with their comparison with ordinary magnesia–alumina bricks, are listed in Table 2. It can be seen that the refractoriness under load of the specially processed magnesia–chrome bricks is significantly improved, and their hydration resistance and thermal shock resistance are increased by more than three times.

It can be seen from Figure 1 that the residual thickness of ordinary magnesia–alumina bricks is very small after 1–2 furnace campaigns, rendering them unfit for further service. In contrast, for the magnesia–chrome bricks after two furnace campaigns, only the working face of the lowest ring bricks within a 1-m width at the very center of the supporting arch-the most severe service area-shows wear of 0–40 mm (Figure 2).

Even after 4–5 furnace campaigns, the residual bricks remain fairly intact (Figure 3). It is evident that the service life of magnesia–chrome bricks still has great potential for improvement.

By using hydration-resistant and thermal-shock-resistant magnesia–chrome bricks, and based on the maintenance standard of "no patching for minor repairs and patching for intermediate repairs-i.e., one new lining for three intermediate repairs (five furnace campaigns) with two patching operations," the original maintenance rate for this area can be reduced from 60% to 30% (Furnaces #4 and #9), with brick consumption reduced by 50%. For Furnaces #6 and #7, the maintenance rate is reduced from 85.2% to 33.3%, and brick consumption is reduced by 60.9%, representing an average reduction of 55.5% in brick consumption.
Several million yuan can be saved annually in the supporting arch and transition zone. When extended to the entire exhaust gas system, the economic benefits are even more substantial. At present, this hydration-resistant and thermal-shock-resistant magnesia–chrome brick is being widely applied.
Microstructure of Hydration-Resistant and Thermal-Shock-Resistant Magnesia-Chrome Bricks
Conventional magnesia–alumina bricks and fired magnesia bricks mainly fail by dusting and spalling. Focusing on improving the refractoriness, hydration resistance, and thermal shock resistance of the products, magnesia–chrome bricks have been developed. These bricks are produced using high-quality magnesia and selected chrome ore as raw materials, through crushing and screening, thorough mixing, high-pressure forming, and ultra-high-temperature firing.
A comparison of their main properties with those of conventional magnesia–alumina bricks is given in Tables 1 and 2. It can be seen that all three developed bricks perform significantly better than conventional magnesia–alumina bricks, with Formula A being the optimum.
The microstructures of conventional magnesia–alumina bricks, conventional fired magnesia bricks, and the high-refractoriness, hydration-resistant, and thermal-shock-resistant magnesia–chrome bricks used in the flue gas system were observed and studied using a Japanese OLYMPUS AHMT3-513NU universal research microscope and a BHS-753P polarizing microscope.
Conventional magnesia–alumina bricks: The aggregate in the bricks consists of conventional magnesia (lower-left and lower-right corners in Figure 4(a)). The periclase main crystals are relatively small, with a considerable portion exhibiting a roe-like morphology. The secondary crystalline phase is a silicate phase dominated by monticellite. A key microstructural feature of conventional magnesia is the thick and continuous silicate film enveloping the periclase phase.
In the matrix of conventional magnesia–alumina bricks (Figure 4(b)), besides periclase and silicate phases, the main crystalline phase is magnesium–aluminum spinel. The spinel in this type of brick is usually concentrated in nests, and individual spinel crystals are often surrounded by silicate phases. Direct bonding between spinel and periclase is rare. However, the bonding between aggregate and matrix is relatively dense (Figure 4(a)).

Conventional fired magnesia bricks:Their mineral phase composition is identical to that of the aggregate portion of conventional magnesia‑alumina bricks. The observation under crossed polarized light is shown in Figure 5. It can be seen that conventional fired magnesia bricks have a simple and dense microstructure.

Hydration-Resistant and Thermal-Shock-Resistant Magnesia-Chrome Bricks: These bricks contain more mineral components and exhibit a more diverse microstructure. The high-quality magnesia aggregate (upper, lower, left, and right parts in Figure 6(a)) has a low silicate phase content and a high direct bonding ratio between periclase phases, forming a dense bond with the matrix.
In the selected chrome ore aggregate (left-center and lower-middle parts in Figure 6(a)), the main crystalline phase is FeCr₂O₄, and the secondary phase is an Mg-containing silicate phase. It is often separated from the matrix by microcracks, whose width and extension length vary with particle size: the larger the particle, the wider and longer the microcracks, and vice versa.
The matrix of the brick is inherently high in purity with a low silicate phase content. Part of the FeO and Cr₂O₃ from the chrome ore diffuses into the periclase crystals, promoting their growth. Meanwhile, some chrome ore reacts with magnesia to form magnesia–chromite spinel between periclase grains, further enhancing the direct bonding between solid phases (periclase–periclase, periclase–spinel, spinel–spinel), as shown in Figure 6(b).

Through the above comparison of microstructures, it can be concluded that the refractoriness, hydration resistance, and thermal shock resistance of magnesia‑chrome bricks are improved compared with conventional magnesia‑alumina bricks and conventional fired magnesia bricks. The mechanism is as follows:
(1) Using high-quality magnesia and selected chrome ore as raw materials, together with high-pressure forming and ultra-high-temperature firing, enables magnesia‑chrome bricks to maintain a high degree of direct bonding between solid phases at high temperatures. They possess sufficient high-temperature strength, excellent volume stability, and resistance to high-temperature creep, thus avoiding deformation and collapse.
(2) The hydration resistance of periclase, magnesium‑aluminum spinel, and magnesium‑chromium spinel increases in the order listed. In magnesia‑chrome bricks, the selected chrome ore itself is a spinel, and it further reacts with magnesia to form magnesium‑chromium spinel, thereby improving the hydration resistance of the product.
(3) The addition of a certain amount of chrome ore grains, with appropriate particle size, forms a controlled number of microcracks in the product (caused by differences in thermal expansion coefficients). These microcracks can absorb energy during the propagation and extension of large spalling cracks, weakening or even terminating their growth, thus improving thermal shock resistance.
Practical Application Comparison
Conventional magnesia–alumina bricks
Conventional magnesia–alumina bricks, whose properties are listed in Table 3, performed in the supporting arch as follows: patching (and sometimes complete replacement) was required after the first furnace campaign (minor repair), and complete replacement was needed after the second furnace campaign (intermediate repair).
For example, Furnace #6 was repaired 9 times per year, including 8 complete replacements and 1 patching of the supporting arch, resulting in a maintenance rate of 94.4%. Furnace #9 was repaired 10 times per year, with 6 complete replacements of the supporting arch, giving a maintenance rate of 60%.
Therefore, prolonging the service life of the brick lining in the flue gas system and reducing brick consumption is urgent.

2. Hydration-Resistant and Thermal-Shock-Resistant Magnesia-Chrome Bricks
The performance of hydration-resistant and thermal-shock-resistant magnesia-chrome bricks used in the supporting arch is as follows: After the first furnace campaign, the bricks remained intact without any patching. After the second furnace campaign, no patching or only minor patching was required.
Although the bricks were still in good condition during intermediate repair and could remain unpatched, patching was carried out within a 1-meter-wide central area to avoid delaying the repair schedule in the next minor repair. Finally, the bricks were replaced after 4–5 furnace campaigns, thus prolonging the service life by 2–3 times.
Conclusion
High-temperature, hydration-resistant, and thermal-shock-resistant magnesia-chrome bricks, developed from high-quality magnesia clinker and selected chrome ore using a special process, have replaced conventional magnesia-alumina bricks and conventional fired magnesia bricks.
Their advantages are as follows: easy on-site construction, good integrity of the brickwork, sufficiently high strength, excellent volume stability and creep resistance, and especially outstanding hydration resistance and thermal shock resistance.
The service life is increased by 2–3 times, and brick consumption is reduced by 55.5%. Savings of several million yuan per year can be achieved in the supporting arch and transition zone alone. At present, this type of hydration-resistant and thermal-shock-resistant magnesia-chrome brick is being widely promoted and applied.