In recent years, the demand fluctuations in the aluminum market have been affected by changes in uncertain factors. To adapt to the fast-paced market changes, quickly start the furnace, provide qualified products, stop the furnace rapidly, and carry out timely maintenance to ensure production operation, higher requirements are put forward for the repair of the furnace lining, especially rapid repair. In order to meet the production needs, maintenance services have been continuously exploring. The selection of materials, including the use of new materials, and the improvement of construction methods, including how to shorten the construction period, have become factors restricting the repair of aluminum smelting furnaces. From furnace shutdown to aluminum liquid production after major maintenance, the shortest cycle of an aluminum smelting furnace is 50 days, and the economic cost of major maintenance of an aluminum smelting furnace is about 55,000 yuan per ton of aluminum.
Taking Japan as an example, in the application of monolithic refractories for furnace repair, the output of monolithic refractories accounted for 34.8% of the total refractory output in 1980, and reached 59.2% in 2000, which has exceeded the output of shaped products. In recent years, monolithic refractories have been more widely used with a higher proportion. The basic structure of the inner lining of an aluminum smelting furnace is shown in Figure 1.

Figure 1 Basic Structure of the Inner Lining of the Aluminum Smelting Furnace
Damage Condition of Aluminum Smelting Furnace
1.1 Forms of Lining Damage
1.1.1 Normal Wear
During the production and operation of the furnace, molten aluminum is repeatedly charged and discharged. When the molten aluminum is heated up, the furnace lining is also heated up accordingly. When new molten aluminum enters the furnace, the furnace lining will be cooled down. The molten aluminum contains substances such as acids and alkalis. During operations such as furnace opening and closing, degassing, and combustion, the furnace comes into contact with various gases, etc. Most refractory materials are multi-component and multi-phase composite systems, and chemical changes will occur during the high-temperature process. After a series of complex processes, various parts of the furnace are damaged to different degrees. When the damage reaches a certain level and affects the continuous operation of safe production, it is necessary to shut down the furnace for lining repair.
Common situations of easy wear:
Furnace door seal, adjustable sealing device, heat-resistant cast iron plate, etc. After long-term use, air leakage points are likely to occur in the seal. Flames flow out along with the air flow. If not repaired in time, the leakage points will become more and more serious, belonging to damage caused by contact with combustion flames;
Furnace threshold: Mechanical wear occurs during degassing or slag skimming operations and feeding operations. In addition, the threshold area has the most contact with the external low temperature and the longest exposure time, and suffers the greatest thermal shock;
Door column: The upper part is similar to the lintel, and the lower part is similar to the furnace threshold;
Lintel: Contact with high-temperature gaseous substances evaporated or sublimated in the furnace, and the position where flames and flue gas overflow;
Upper furnace wall: Splashing of molten aluminum and erosion by various high-temperature gaseous compounds;
Lower furnace wall and molten pool: Scouring by molten aluminum, corrosion by impurities, impact of temperature changes, and impact of materials;
Slag line: The harshest environment area, with wave impact on the molten aluminum surface, adhesion of alkaline debris, various furnace gases, impact of temperature changes, etc.;
Furnace roof: Impact by the pressure of combustion gases and vibration impact of top equipment, etc.
1.1.2 Abnormal Damage
There are also many types of abnormal damage to aluminum smelting furnaces, including mechanical impact, mistakes in inputting production process parameters, early damage caused by repeated furnace startup and shutdown, and damage caused by too fast temperature rise and fall during furnace startup and shutdown. For example, in a workshop, when a forklift was feeding materials into furnace No. H, the door column castable was damaged by impact, resulting in easy fire leakage after the furnace door was closed. Finally, the furnace was shut down, the damaged part was removed, and re-casting was carried out. In short, damage is an inevitable phenomenon. Regardless of external or internal reasons, abnormal damage should be prevented during production operation, and production should be controlled in accordance with the production process technology to ensure that the furnace lining is subject to slow and normal wear.
1.2 Influencing Factors of Lining Damage
1.2.1 Poor Material Suitability
In the design of the aluminum smelting furnace lining, through the input of working condition information, the materials selected for design can meet the usage requirements to a certain extent and within a certain special range. From design to production and use, through a series of processes, the performance of the materials will more or less decrease within the performance range. In actual production, for the same furnace type and the same process, the damage conditions are different. For the index categories emphasized in the material design, in accordance with the requirements of national and industry standards, sometimes materials with large differences only meet the lower limit value in individual indexes, which leads to unstable quality of the furnace lining. A company's 25T aluminum smelting furnace undertakes process procedures such as charging, melting, heating up, slag skimming, and transferring molten aluminum during the aluminum processing production process. In the company's aluminum smelting furnace, the area at the lower mouth of the burner has quality problems due to poor material performance, and the damage is shown in Figure 2.

Figure 2 Damage to the Area at the Lower Mouth of the Burner of the Aluminum Smelting Furnace
1.2.2 Quality Risks in Construction Technology
The construction of the furnace lining is a concealed engineering project. When acceptance is not timely or strict, unknown quality risks may be hidden. Concealed engineering refers to the construction that will be covered by subsequent processes, and its specific conditions cannot be observed from the appearance. Therefore, the materials for concealed engineering need to be confirmed before construction, as they cannot be detected after completion. If inferior materials are used, safety risks are extremely likely to occur.
Under normal circumstances, due to various influencing factors, the following quality problems may arise:
The materials for each part of the furnace lining structure are not used as per design requirements. When construction personnel lack a sense of responsibility, they may fail to use materials matching the furnace lining structure as designed, or substitute materials with similar properties;
During construction, the operational skills of construction personnel are insufficient. Although the masonry and castings meet technical specifications, the overall requirements are not met;
The masonry or castings during construction fail to meet the acceptance standards, resulting in low qualification rates and overall poor quality;
The equipment configuration is insufficient, including the precision of brick cutting machines, cutting machines, the efficiency of mixers, and the mixing effect of mixers.
Determination of Repair Methods
After the furnace is shut down, inspect the furnace body. According to the different damaged parts of the furnace lining, the furnace building materials used vary depending on the location. Check the extent of damage, the size of the surrounding damaged area, and the depth of damage to determine the preliminary size of the furnace excavation area. Re-judge the affected area based on the furnace excavation situation until the completion of furnace excavation is confirmed.
2.1 Forms of Lining Damage
The main damage forms of each part of the lining are statistically shown in Table 1.
| Position Name | Burner | Upper Furnace Wall | Furnace Roof | Column Lintel | Furnace Threshold | Impermeable Layer | Furnace Bottom | Lower Furnace Wall |
|---|---|---|---|---|---|---|---|---|
| Brief Description of Damage | High - temperature Oxidation | Splash Corrosion | Falling - off | High - temperature Oxidation | Wear | Leakage | Deposition | Corrosion |
2.2 Degree of Damage
The degree of damage to the furnace lining is usually determined by looking at the degree of corrosion, the area of the damaged surface region, and the depth of damage. During the process of removing the damaged parts by digging out, check whether the transition zone around the damaged area is damaged and whether it needs to be dug out. In the repair process, it is hoped that the construction period is short, the cost is low, and the service life of the overall lining is not affected. Therefore, choosing local repair becomes the preferred method. Based on the on-site damaged position and the degree of damage, determine which material to use (a material that is better than or the same as the originally used material), and which construction process route to adopt, so as to form a construction technical plan.
Main Factors Affecting Local Repair
3.1 Requirements for Protective Furnace Dismantling
Generally, a small pneumatic pick or an electric pick is used to remove the damaged part of the furnace lining. The pneumatic pick is required to have a high impact frequency and a small amplitude, so as to have a small impact on the overall furnace body and avoid damaging the surrounding furnace body and expanding the repair area. After removing the damaged area, check the anchoring property of the bonding surface between the original body area and the repair area, and clean up the residue to make the bonding surface clean.
3.2 Selection of Repair Materials
Select repair materials according to different parts of the furnace lining, because the working conditions of the furnace lining in different parts are different. In addition, analyze the cause of damage at the damaged point, and take measures to prevent the damage from occurring again. Measures can be taken to improve the performance of the repair material. Generally speaking, a better material than the original body is used for repair.
3.3 Complexity of Structural Positions
In the construction and repair of the furnace lining, starting from the basic structure of the furnace, for positions such as the furnace bottom, furnace wall, and furnace roof, in addition to different materials, the formwork support methods are also different, and the difficulty of pouring is also different. In particular, when the working surface of the furnace wall is poured with unshaped refractory materials, the entire castable may have a larger or smaller cross-sectional thickness, which will affect the later scalability, bondability, etc. The pouring port needs to be set properly during pouring, including considering the position that the vibrator can reach when inserted. When the area of the pouring region is large, it should be poured in blocks, as shown in Figure 3.

Figure 3 Block - by - block Pouring of the Furnace Body
Optimized Control Measures
4.1 Inspection after Excavation of Repair Area
When excavating and cleaning the repair area for the lining repair of the original furnace body, a small pneumatic pick shall be used, with judgment conducted simultaneously during excavation. Inspection of the original body around the repair area and the bonding surface is particularly critical. In practice, two control principles should be adhered to:
① The damage degree of the original body around the repair area after excavation shall not have continuous cracks or closed-loop cracks;
② The original body and the new body shall have good anchoring properties, and the bonding surface shall form an irregular, randomly uneven rough surface, and anchoring hooks shall be installed if necessary.
4.2 Control of Construction Technology Requirements
During construction of any part of the furnace lining, thermal insulation and refractory materials shall be laid by masonry, and inspection and acceptance shall be carried out in accordance with the furnace construction code GB50211 - 2014³ and the design requirements of the furnace. The inspection of bricks mainly refers to on-site inspection of refractory brick dimensions, appearance, fusion holes, chipped edges, missing corners, cracks, and distortion, excluding inspection of chemical composition, thermal properties, and mechanical properties. The inspection method shall comply with the provisions of the national standard GB10326 - 2001⁴.
For monolithic refractory casting, the on-site inspection and acceptance of monolithic refractories mainly focus on whether they are within the valid period. Generally, monolithic castables are mixed with water according to the water ratio specified in the product manual. The bonding methods of common refractory materials are divided into water bonding, chemical bonding, polymeric bonding, and coagulation bonding, etc. A company uses castables with water bonding. When there is any dispute, sampling can be sent to a qualified inspection department for identification. For example, in a certain aluminum smelting furnace, an amorphous refractory material newly developed by Company A was used in this area, and the comparison between the required and measured physical and chemical indicators is shown in Table 2.
During casting construction, in accordance with the material usage requirements, the water - cement ratio, mixing time, uniform mixing, material cleanliness shall be ensured, the vibration force and time shall be controlled, and appropriate setting accelerators or retarders shall be added to control the initial setting and formwork removal time.
| Serial Number | Physical and Chemical Indicators Tested | Unit | Index Requirement | Third - Party Inspection Report |
|---|---|---|---|---|
| 1 | Chemical Composition - Al₂O₃ |
% | ≥77 | 78.26 |
| - SiO₂ | % | ≤16 | 13.5 | |
| 2 | Bulk Density - 110 °C×24 h |
g/cm³ | ≥2.39 | 2.76 |
| - 815 °C×3 h | g/cm³ | ≥2.5 | 2.7 | |
| 3 | Compressive Strength - 110 °C×24 h |
MPa | ≥70 | 76 |
| - 815 °C×3 h | MPa | ≥65 | 67.5 | |
| 4 | Refractoriness Under Load - 0.2 MPa, T4.0 |
°C | ≥1300 | 1371 |
| 5 | Flexural Strength - 110 °C×24 h |
MPa | ≥10 | 20.7 |
| - 815 °C×3 h | MPa | ≥8 | 17 |
Table 2 Comparison between Required and Measured Physical and Chemical Indices of Monolithic Refractories
It can be seen from Table 2 that for the monolithic refractory castable used for side wall repair, the 9 physical and chemical indexes submitted for third - party testing meet the requirements and can be used.
4.3 Maintenance and Oven - drying Control
For furnaces repaired with monolithic refractories, the self - heating maintenance time is usually not less than 24 hours. The overall oven - drying temperature - rising curve is formulated according to the furnace type for oven - drying. Generally, the furnace is continuously dried for 4 to 10 days. Combined with the characteristics of the repair area, the water - draining and heat - preserving time in the three stages during the oven - drying process and the temperature in this period are adjusted to ensure the cohesiveness of the repair area and the comprehensive performance in later use. The combustion system on the furnace itself is directly used for baking. According to the temperature - rising curve, the purpose of baking is achieved. It should be noted that before ignition, the air in the pipeline should be exhausted before ignition.
Application Effect
5.1 Shortened Repair Period
In the past, during the repair of aluminum smelting furnaces, extensive repair methods were adopted, resulting in a large demolition area. Minor repairs were often upgraded to medium - scale repairs, and medium - scale repairs to major overhauls. This consumed a significant amount of construction time, making it difficult to meet production requirements and affecting the completion of production orders.
By adopting efficient local repair, the repair period can be shortened. Conventionally, for a 30t furnace, major and medium - scale repairs take an average of 30 days (approximately 45 days for major overhauls and 16 days for medium - scale repairs), while minor repairs require about 15 days, achieving a reduction of approximately 10 days. After the furnace shutdown, through local protective excavation and cleaning, an area of approximately 3m² was repaired, which was completed in 4 shifts.
Construction and transformation were carried out strictly in accordance with the relevant standards and requirements of the Code for Construction and Acceptance of Industrial Furnace Masonry Works, with strict quality control throughout the process. The transformation was successfully completed and passed the acceptance inspection. The external appearance before and after the transformation is shown in Figure 4.

Figure 4 Effect of Local Repair of Aluminum Smelting Furnace
5.2 Improved Repair Quality
In terms of material compatibility, with the extensive introduction of new materials and technologies, local repair has reduced construction difficulties. In the formwork design, the principles of simplicity, efficiency, and ease of disassembly and assembly are adhered to. For example, in a certain aluminum smelting furnace, newly developed materials were used in the repair area.
By strictly following the casting construction requirements, such as weighing water addition, controlling mixing time, vibration time, and environmental hygiene, the qualified rate of concealed acceptance for the casting process quality was ensured to be 100%. Meanwhile, in subsequent production, it guaranteed production continuity and helped extend the overall service life of the furnace lining.
The application of this repair method has realized local repair of the aluminum smelting furnace lining. Through year - on - year comparison, local repairs of aluminum smelting furnaces have gradually decreased, from 63 maintenance items in 2022 to 44 in 2023, a reduction of 30.1%. The application of this process technology has achieved certain results.
Conclusion
1) The adoption of efficient local repair can shorten the repair period by about 10 days.
2) The extensive introduction of new materials and technologies not only reduces construction difficulties, but also ensures that the qualified rate of concealed acceptance for the casting process quality can reach 100%.
3) After the application of local repair technology, repairs have gradually decreased year by year, with maintenance items decreasing by 30.1% year on year, demonstrating the effectiveness of the technology.