Research And Application Of Low Thermal Conductivity Magnesium-aluminum Spinel Bricks Heat Insulation Performance

May 15, 2025

Leave a message

 

Research and application of low thermal conductivity magnesium-aluminum spinel bricks heat insulation performance

 

Abstract: In order to solve the problem of high thermal conductivity of magnesium-aluminum spinel bricks, the sintering properties and microstructure of rare earth oxide-doped porous magnesium-aluminum spinel refractory aggregate were studied. Industrial α-alumina micropowder and electrofused magnesia sand were used as the main raw materials, sodium dodecylbenzene sulfonate (SDBS) was used as the blowing agent, and dextrin was used as the binding agent to prepare porous magnesia-aluminum spinel, in addition to the addition of different mass fractions of Y2O3, Yb2O3, La2O3, and Sm2O3, respectively, and sintered at 1600 ℃ with a heat preservation of 3h, respectively, and the samples were determined by sintering the bulk density, apparent porosity, and the sintered samples by XRD, SEM, EDS and other means of characterization of its physical phase composition and microstructure, in order to reveal the rare earth oxides on the porous magnesium-aluminum spinel sintering reaction process mechanism. The introduction of rare earth oxides on the sintering of magnesium-aluminum spinel has a promotional effect, the bulk density of the sample, compressive strength of the sample in the Sm3O2 addition of 1.5wt% reached a maximum, respectively, 2.28g/cm³ and 50.5Mpa. rare earth oxides with magnesium-aluminum spinel to form a replacement solid solution, thereby promoting the sintering of magnesium-aluminum spinel densification, the cationic vacancies and the magnesium-aluminum spinel crystal lattice defects. Favorable to the development and growth of magnesium-aluminum spinel crystals, through the products made of this raw material has a significant reduction in thermal conductivity than similar products.

 

1.Preamble

 

At present, China's cement rotary kiln energy consumption is very serious, especially the existing cement rotary kiln before and after the transition zone refractory materials without the protection of the kiln skin, refractory bricks are directly subject to material erosion, thermal load and mechanical stress impact, the use of very harsh conditions. At present, China's large-scale cement rotary kiln transition zone generally use silica brick, silica red brick or magnesia-aluminum spinel brick, service life basically meet the requirements of cement production. However, due to magnesium-aluminum spinel brick and silica brick, silica red brick thermal conductivity, magnesium-aluminum spinel brick ≥ 3.0 W/m-K, silica brick ≥ 2.8 W/m-K, resulting in cement rotary kiln operation process before and after the transition zone cylinder wall temperature is too high, an average of 340 ℃ or so, up to 400 ℃. Higher cylinder wall temperature brings a series of problems, such as increasing coal consumption of cement tons of clinker, increasing the emission of polluting gases, and seriously cause "red kiln", affecting the safe operation of cement rotary kiln.

 

Refractory lightweight mainly through the introduction of a certain amount of pores into the material, without significantly reducing the strength of the refractory material at the same time, has a lower thermal conductivity; in energy saving at the same time can also reduce the consumption of resources in the process of raw material preparation and service, is a direction of the research and development of refractory materials. Therefore, the development of new low thermal conductivity magnesia-aluminum spinel lightweight refractories is of great practical significance for energy saving and consumption reduction in the cement industry.

 

2.Test

 

2.1Test material

 

For the test, alumina (particle size ≤0.088 mm) and electrofused magnesia (particle size ≤0.088 mm) were selected as the main raw materials (the chemical composition is shown in Table 1), sodium dodecylbenzene sulfonate (SDBS) as the blowing agent, dextrin as the stabilizer of the foam, and yttrium oxide (Y2O3), ytterbium oxide (Yb2O3), lanthanum oxide (La2O3) and samarium oxide (Sm2O3) as the additives.

 

1

Table 1 Chemical composition of raw materials

 

2.2 Test Formulation and Sample Preparation

 

Alumina and electrofused magnesium sand mixed with 1:1 (molar ratio), rare earth oxides as additives, and then add 35% of water, 0.01 wt% foaming agent and 0.1 wt% foam stabilizer, the prepared slurry into the mixer for 5 min, poured into the 40 mm × 40 mm × 40 mm molds, in the process of pouring molds should be loaded with materials and pounding, fill the molds with full of material after the mold on the The test formula is shown in Table 2.

 

2

Table 2 Experimental formulations (wt%)

 

2.3 Specimen handling and performance testing

 

After molding, the specimens were dried naturally for 24 h, and then demolded into a drying box at 110°C for 12 h. Finally, the dried specimens were calcined at 1600°C for 3 h. The physical composition was analyzed using an X-ray diffraction analyzer (PANalytical X'pert Powder Diffractometer) and the bulk density, apparent porosity, and room temperature compressive strength of the specimens were measured, respectively. The bulk density, apparent porosity, and room temperature compressive strength of the specimens were measured.

 

3.Analysis and Discussion of Experimental Results

 

3

Fig. 1 Relationship between different rare earth oxides and bulk density and apparent porosity of specimens

 

The effects of different rare earth oxides on the bulk density and apparent porosity of magnesium-aluminum spinel lightweight aggregate are shown in Figure 1. As can be seen from the figure, the sample without added rare earth oxides mineralizer has the lowest bulk density, and all four rare earth oxides have the effect of promoting the sintering of the sample. The sample with the addition of Sm2O3 had the highest bulk density and the lowest apparent porosity of 2.15 g/cm³ and 35.27%, respectively. When 1 wt% of Yb2O3 was added, the samples had relatively high bulk density and apparent porosity of 2.13 g/cm³ and 47.77%, respectively.

 

5

Fig. 2 Effect of different rare earth oxides on compressive strength of specimens at room temperature

 

The effects of different rare earth oxides on the compressive strength of the specimens are shown in Fig. 2. From the figure, it can be seen that the addition of rare earth oxides is conducive to improving the compressive strength of Mg-Al spinel lightweight aggregate, and the compressive strength is the highest when the addition of Sm2O3 is 1 wt%, which reaches 46.8 MPa. This is mainly due to the fact that the sintering-promoting property of Sm2O3 is the best, and the result is also consistent with the results of the bulk density test.

 

6

Fig. 3 X-ray diffraction patterns of specimens with different rare earth oxide additives

 

The X-ray diffraction patterns of the specimens with 1 wt% content of different kinds of rare earth oxides are shown in Fig. 3. The specimens without added rare earth oxides showed intense diffraction peaks attributed to MgO at around 46°. In contrast, the MgO diffraction peaks at 46° in the samples doped with Y2O3, Sm2O3 and La2O3 are obviously weakened or even disappeared, indicating that the development and formation of MgAl2O4 is more complete in these three samples. It is worth noting that in the Yb2O3 sample, the diffraction peak at 46° is still obvious, which shows that the sintering-promoting effect of Yb2O3 is poorer than that of the other three rare earth oxides.

 

In summary of the results, it can be seen that the addition of rare earth oxides as mineralizing agents can effectively promote the formation of MgAl2O4, in which the samples with the addition of Sm2O3 have relatively high bulk density and compressive strength. Therefore, the effect of the addition of Sm2O3 on the bulk density and apparent porosity of the specimens was specifically investigated, and the results are shown in Fig. 4.

4

Fig. 4 Effect of different Sm2O3 additions on apparent porosity and bulk density of specimens

 

The relationship between Sm2O3 addition and the apparent porosity and bulk density of the specimens is shown in Fig. 4. From the figure, it can be seen that the variation trends of apparent porosity and bulk density are opposite. With the increasing of samarium oxide content in the specimen, the apparent porosity decreases and the bulk density increases with the increase of the amount of samarium oxide in the range of 0~1.5 wt%. When the samarium oxide content was 1.5 wt%, the porosity was the lowest and the bulk density was the highest. However, when the samarium oxide content exceeded 1.5 wt%, the apparent porosity began to increase and the bulk density began to decrease.

 

5

Fig. 5 Effect of different contents of Sm2O3 on the compressive strength of specimens at room temperature

 

The relationship between different samarium oxide contents and the room temperature compressive strength of the specimens is shown in Fig. 5. As can be seen from the figure, when the samarium oxide content in the specimen is in the range of 0~1.5wt%, the normal temperature compressive strength of the specimen is proportional to the change of samarium oxide content. When the samarium oxide content is 1.5 wt%, the compressive strength of the specimen is the maximum value, which is 94% higher than that of the specimen without samarium oxide. However, when the samarium oxide content exceeded 1.5 wt%, the compressive strength at room temperature began to decrease. It shows that the addition of samarium oxide can improve the compressive strength of Mg-AlSe lightweight aggregate.

 

XRD of the samples with different contents of Sm2O3 added, the prepared samples have strong MgAl2O4 diffraction peaks. Comparison with the diffractograms of the specimens without additives in Fig. 3 reveals that the MgO diffraction peaks of the Sm2O3-containing specimens are relatively flat, among which the diffraction peaks of magnesium oxide are the most flat when the Sm2O3 addition is 1.5 wt%. This shows that the addition of Sm2O3 can promote the formation of magnesium-aluminum spinel. It is also worth noting that at 34.2° and 23.7° (1.5 wt%), Sm2O3 reacted with the impurities in the raw material to generate a high melting point rare earth silicate phase Ca2Sm8(SiO4)6O2 replacing the original low melting point silicate glass image, which is helpful for the sintering properties and high temperature properties of the material. The magnesium-aluminum spinel peaks and magnesite peaks of the prepared samples were shifted to a certain extent, which was mainly due to the 4f electron-layer structure and chemical activity of the rare-earth ion Sm3+ (r = 0.0964 nm) that caused solid solution of the particles, lattice distortion, and lattice activation, which ultimately promoted the sintering.

 

4. Conclusion

 

In the synthesis of Mg-Al spinel lightweight aggregate, the addition of yttrium oxide, ytterbium oxide, lanthanum oxide and samarium oxide can increase the bulk density, decrease the apparent porosity, increase the compressive strength, and promote the formation of Mg-Al spinel, of which the sintering performance of the samarium oxide samples is more favorable. When the addition of Sm2O3 reaches 1.5 wt%, the sample has the lowest porosity and the highest bulk density of 2.28 g/cm³ and 31.72%, respectively.

 

5.Applications

 

Through the above technology, low thermal conductivity multi-layer composite magnesium-aluminum spinel bricks are applied in 24-32 meters, the average temperature is 43℃ lower than that of magnesium-aluminum spinel bricks, and the service life reaches more than 12 months. Low thermal conductivity magnesium-aluminum spinel bricks are not only recognized by the customers domestically, but also have been applied in many rotary kilns by overseas customers such as Mexico Cement and Turkey, and have been highly praised.

 

Aiming at the problems of high energy consumption and high carbon emission in the cement industry, the low thermal conductivity multilayer composite magnesia-alumina spinel bricks have the following advanced features: the optimization of the working layer through the form of a three-layer composite structure reduces the thermal conductivity of the working layer and improves the resistance to thermal shock, while at the same time optimizing the heat-insulating layer and improving the strength of the insulation layer. Zirconia-reinforced alumina fiber board with excellent high temperature resistance was selected as the material for the thermal insulation layer through the study of different thermal insulation materials. During the preparation process, the innovative production process is used to realize simultaneous molding and firing, simplify the process, reduce the cost and improve the production efficiency. Low thermal conductivity magnesium-aluminum spinel bricks thermal conductivity 2.4-2.5W/(m-K) is far lower than the current market ordinary magnesium-aluminum spinel bricks 3.0-3.3W/(m-K).

 

Through the actual application of customer feedback low thermal conductivity multi-layer composite magnesium-aluminum spinel bricks can effectively reduce the temperature of the cylinder on the transition zone of the cement kiln, energy saving and carbon reduction benefits. For the cement rotary kiln energy saving and emission reduction provides a new direction.

 

modular-1
Zinfon Refractory Technology Co.,Ltd

We are a refractory material supplier integrating R&D,production,construction,warehousing and commerce.

We are offering various magnesia and alumina refractories including both shaped and unshaped products, raw materials and related chemical products.

We are certified to ISO9001, ISO14001, ISO45001 and other national and local certifications as follows: