Properties that ladle purge bricks should possess
To meet the above metallurgical functions, purge bricks must possess the following main properties:
(1) Good gas permeability. Gas permeability is one of the important parameters for measuring the quality of purge bricks. Studies have shown that the stirring energy of molten steel is directly proportional to the flow rate of the blown gas; stirring energy directly affects the stirring efficiency of molten steel, and only sufficient stirring can achieve good stirring results. When the argon blowing volume is constant, the more argon bubbles blown out, the more favorable it is for the degassing and stirring of molten steel.
(2) High-temperature corrosion resistance. Refining ladles have very strict requirements in terms of temperature and time, with the maximum temperature often exceeding 1750°C and the refining time sometimes reaching dozens of minutes. During refining operations, the basicity of the slag has a great impact on the service life of purge bricks. Therefore, purge bricks are eroded by highly permeable alkaline slag at high temperatures, leading to rapid degradation.
(3) High-temperature wear resistance. When argon is blown from the bottom of the refining ladle, the flow rate of molten steel in the ladle is very high due to the bottom argon blowing, significantly increasing the scouring and wear of the molten steel on the lining materials, bottom purge bricks, and seat bricks. During ladle hot repair, in order to remove the residual steel and slag on the surface of the purge bricks and restore their gas permeability, oxygen blowing cleaning is required to melt the steel slag adhering to the surface of the purge bricks; at the same time, blowing gas into the purge bricks to remove the molten slag. During the cleaning process, the purge bricks are eroded by high-speed gas flows, so they are required to have good high-temperature wear resistance.
(4) Good thermal shock resistance. Due to the intermittent operation of the ladle, when molten steel is poured into the ladle, the end of the purge brick is affected by high-temperature molten steel, causing a sudden temperature rise. When blowing argon, the material is cooled by cold gas flow, generating large thermal stresses inside the material. At the same time, significant temperature changes also occur when molten steel is poured into an empty ladle, so the service conditions of purge bricks are extremely harsh, making them prone to thermal spalling and structural spalling.
(5) Simple installation and safe and reliable operation. Purge bricks are installed inside the seat bricks at the bottom of the ladle, and their working conditions are extremely harsh. The service life of ladle purge bricks cannot be synchronized with the entire ladle life, so they need to be replaced. Therefore, simple installation operation and safe and reliable use are required to avoid steel penetration and leakage incidents.
Common Classification of Ladle Purge Bricks
After years of development, purge bricks commonly have three main structural types: diffusion type, slit type, and straight-through hole type.
1. Diffusion Type Purge Bricks
This is the earliest form of purge bricks. Due to the high porosity of the material itself, the large number of pores provide channels for inert gases. However, the disadvantages of this surface-porous diffusion-type purge brick include low strength, poor erosion resistance, easy spalling caused by penetration of molten steel and slag, and poor stirring effect on molten steel. It is rarely used in domestic ladle purge bricks today.
2. Slit Type Purge Bricks
There are two forms of slit-type purge bricks:
Joint Assembly Type: The central part of the purge brick is formed by assembling several shaped thin plates to create slits, with the exterior cast using castable material. The disadvantage of this "joint assembly" type is poor controllability of the blown gas.
Precast Slit Type: Dozens of straight-through slits are precast into the brick body, commonly known as the "slit type". Compared with the joint assembly type, slit-type purge bricks offer advantages such as longer service life, higher gas blowing efficiency, larger gas flow rate, and better stirring effect.
3. Straight-Through Hole Type Purge Bricks
These are made by embedding varying numbers of thin steel pipes into the brick, with gas channels composed of many straight micro-pipes, formed by casting. Compared with diffusion-type purge bricks, straight-through hole type purge bricks have a 2–3 times longer service life and better stirring effect. However, their drawback is the limited gas flow they can provide. In the later stages of use, refining failures often occur due to reduced gas permeability or blocked gas flow.
Installation Methods of Ladle Purge Bricks
The installation of purge bricks can be categorized into two types: internal installation and external installation.
Internal Installation
In this method, the purge brick is pre-assembled with the seat brick outside the ladle. During ladle lining construction:
The area at the ladle bottom for the purge brick is cleaned.
After laying the curtain bricks, the pre-assembled purge brick with its seat brick is hoisted into position.
The ladle bottom and lining are then sequentially built up.
External Installation
This type consists of a seat brick, sleeve brick, and purge brick. The process involves:
Installing the seat brick at the ladle bottom during initial lining.
Constructing the ladle bottom and walls.
Applying fireclay evenly to the outer surfaces of the sleeve brick and purge brick, then forcefully inserting them into the seat brick.
Sealing the bottom with backing bricks, attaching a flange, and baking the assembly.
Application Scenarios
Internal Installation is used when the service life of the ladle lining matches that of the purge brick. However, it is less common today due to lower safety, poor reliability, and difficult replacement procedures.
External Installation is preferred for scenarios requiring frequent purge brick changes. It offers easier maintenance and higher operational safety, making it the standard choice for modern ladles.
Common Materials of Ladle Purge Bricks
At present, the materials of purge bricks include corundum, chrome corundum, high-alumina, and magnesia-chrome, etc.
A. Corundum-spinel system purge bricks
The slag resistance and thermal shock resistance of single-phase corundum castables for purge bricks are not ideal, while spinel materials have good slag erosion resistance. According to the principle of improving refractory performance through composite modification, high-purity electrofused spinel is added to corundum castables to enhance their properties. The raw materials include tabular corundum as granular material, electrofused white corundum, spinel, active α-Al₂O₃ micro-powder, etc., as fine powders, and calcium aluminate cement as the binder.
Advantages: Significantly improved thermal shock resistance and slag resistance.
Disadvantages: During high-temperature treatment, spinel undergoes volume changes, leading to poor volume stability of the purge brick, which is difficult to control in the production process.
B. Corundum-chromium oxide system purge bricks
To further improve the erosion resistance of purge bricks against steel slag, a certain amount of chromium oxide micro-powder is added to the product. The main raw materials are tabular corundum as granular material, tabular corundum fine powder and chromium oxide micro-powder as fine powders, and calcium aluminate cement as the binder. At high temperatures, chromium oxide and aluminum oxide form a high-temperature solid solution, while forming a partial solid solution of MgO·Cr₂O₃-MgO·Al₂O₃ with a small amount of magnesium oxide. This solid solution significantly enhances the resistance to erosion by Fe₂O₃ or slag, and has a very high viscosity, effectively preventing the penetration and erosion of steel slag at high temperatures. Meanwhile, a small amount of Cr₂O₃ can inhibit excessive growth of Al₂O₃ and reduce internal stress in crystals, improving the physical properties of the material.
Disadvantages: Excessive addition of Cr₂O₃ will severely inhibit the growth of corundum crystals, generating internal stress and reducing the material's physical properties. Additionally, Cr₂O₃ is costly, and excessive addition significantly increases costs; moreover, Cr₂O₃ causes serious environmental pollution.
C. Corundum-spinel system purge seat bricks
Corundum-spinel system purge seat bricks are the most widely used material, mainly composed of tabular corundum, α-Al₂O₃ micro-powder, and spinel, bonded with pure calcium aluminate cement.
Advantages: Spinel has strong resistance to acids and alkalis and is a high-melting-point compound with excellent properties. Aluminomagnesium spinel has strong resistance to basic slag and is stable against iron oxides. It reacts with magnetite at high temperatures to form a solid solution, improving the high-temperature corrosion resistance of the purge seat brick. Meanwhile, spinel solid-dissolved with MgO or Al₂O₃ has better thermal shock resistance due to the difference in expansion coefficients between minerals.
Disadvantages: When MgO and Al₂O₃ form spinel according to the theoretical composition, about 8% volume expansion occurs, making it difficult to densify during firing and hard to control the volume change of the purge seat brick.
D. Corundum-chromium oxide system purge seat bricks
Corundum-chromium oxide system purge seat bricks are developed based on the corundum-spinel system to improve the high-temperature spalling resistance of purge seat bricks. The main raw materials include tabular corundum, α-Al₂O₃ micro-powder, industrial chromium oxide, and spinel, bonded with pure calcium aluminate cement.
Advantages: On the basis of spinel improving the performance of seat bricks, the solid solution formed by Al₂O₃-Cr₂O₃ significantly enhances the resistance to erosion by iron oxide slag. Adding a small amount of Cr₂O₃ inhibits excessive growth of alumina crystals, reducing internal crystal stress and improving the thermal shock resistance, erosion resistance, and scouring resistance of the purge seat brick.
Disadvantages: Excessive addition of Cr₂O₃ seriously affects the growth rate of corundum crystals, reducing the material's physical properties. Additionally, Cr₂O₃ causes serious environmental pollution, contradicting the national requirements for sustainable development.
Damage Mechanism of Ladle Purge Bricks
The operation of purge bricks is discontinuous, and different physical and chemical erosion damages occur at different times during the entire ladle ladle turnover cycle. In practice, the damage to purge bricks can be classified as follows:
(1) Oxygen Burning and Cleaning Effect
After the ladle is tapped and before receiving steel again, the ladle undergoes hot repair in the hot repair zone. During this time, oxygen burning and cleaning are used on the working surface of the purge brick to remove residual steel and slag. This measure is beneficial for the normal use of the purge brick, as it ensures the cleanliness of the working surface and the unobstructed gas channels, allowing the ladle turnover cycle to proceed smoothly. However, it is difficult to accurately determine the thickness of residual steel and slag on the working surface of the purge seat brick in the hot repair zone. Therefore, after removing the residues, accidental burning of the purge brick may occur, which can be more severe when the bottom condition of the ladle is poor or the hot repair operator misjudges. The temperature during oxygen burning can exceed 2000°C, and the high-temperature gas flow is extremely damaging to the purge brick. The melting loss in these few minutes is often 2-3 times higher than the normal refining erosion loss.
(2) Mechanical Wear Effect
During the tapping process, the high-speed and strong scouring of molten steel on the bottom of the ladle also accelerates the erosion of purge bricks. Studies on purge brick erosion through hydraulic model tests have found that when low-velocity gas flow is injected into the liquid molten pool, the gas flow rebounds and hits the front of the purge brick, exerting a certain impact force on the refractory material around the gas outlet. When the gas flow rate is further increased, the reverse pulse frequency decreases, but the reverse impact intensity increases. Additionally, when argon blowing enters the normal spray state, a strong bubble-forming gas jet bundle is created, which enhances the stirring at the bottom of the ladle and intensifies the liquid phase movement. The two-phase turbulent flow subjects the purge brick to strong shear and impact stresses. When the purge brick is higher than the seat brick, it is particularly susceptible to shear and scouring from this turbulent flow, and the part above the seat brick is generally eroded away after one use. This is especially likely to occur when a new purge brick is replaced. Furthermore, rapid closure of the valve after refining ends can cause reverse impact of molten steel, accelerating purge brick damage.
(3) Thermal Stress Effect
The refractory material on the working surface of the purge brick, especially around the gas outlet, is directly exposed to high-temperature molten steel and cold gas flow, resulting in a large temperature gradient. Due to multiple uses, the purge brick undergoes significant thermal shock, particularly in the area near the gas outlet, where thermal stress is greater, making it prone to annular cracks and fracture.
(4) Chemical Erosion Effect
The working surface of the purge brick is in long-term contact with slag and molten steel. During the entire ladle campaign, the slag continuously infiltrates and penetrates into the brick. Oxides such as MnO, MgO, SiO₂, FeO, and Fe₂O₃ in the molten steel and slag react with the brick:
12CaO+7Al2O312CaO⋅7Al2O3
FeO+Al2O3FeO⋅Al2O3
2MnO+SiO2+Al2O32(MnO)⋅SiO2⋅Al2O3
The low-melting-point products such as FeO·Al₂O₃, 2(MnO)⋅SiO2⋅Al2O3, and 12CaO⋅7Al2O3 are scoured away, causing erosion of the purge brick.
Approaches to Improve the Service Life of Ladle Purge Bricks
The approaches to improve its service life are as follows:
(1) Adding zirconium-based materials and tabular corundum to enhance the spalling resistance of purge bricks.
(2) Optimizing the selection of ultrafine powders.
(3) The stirring intensity of molten steel is directly proportional to the argon blowing volume.
(4) Uniform material distribution to improve the volume stability of purge bricks.
In addition to the above points, the following measures can also be referenced to improve the service life of ladle purge bricks:
Optimize Purge Brick Design and Materials
Adjust the materials and structure of purge bricks to enhance their erosion resistance. For example, adding large-particle aggregates to purge bricks can improve their wear resistance.
Develop integral double-core ladle purge bricks. When one gas core reaches the end of its service life, the gas valve can be switched to the other gas core for continuous use, thereby extending the overall service life of the purge brick.
Improve Installation and Lining Methods
Ensure standardized installation operations for purge bricks to avoid local suspension and misalignment.
Thoroughly clean debris from the ladle shell before installation, and use fireclay or other padding materials to level the bottom to prevent local suspension at the bottom of the seat brick.
Leave appropriate gaps during ladle bottom lining and fill them with suitable gap-filling materials to reduce the impact of expansion on the seat brick.
Control Reasonable Bottom Blowing Parameters
Excessively high bottom blowing pressure will cause violent rolling of molten steel, increasing the chance of contact between molten steel and air and leading to secondary oxidation; excessively low pressure will cause bottom blowing failure and affect metallurgical effects. Therefore, reasonable control of bottom blowing parameters is key to improving the service life of purge bricks.
Regular Maintenance and Inspection
Regularly inspect and maintain the bottom blowing device to prevent air leakage and gas loss.
Timely replace damaged components to avoid production interruptions and cost increases caused by equipment failures.
Optimize the Service Environment of Purge Bricks
Reduce erosion on refractories by optimizing the service environment of purge bricks. For example, optimizing ladle refractories, adjusting purge brick materials, and changing external shapes can improve the erosion resistance of ladles and thus extend their service life.