What is low-cement refractory castable?

 

 Low-cement refractory castables refer to castables bonded with calcium aluminate cement where the CaO content is less than 2.5%, meaning the amount of calcium aluminate cement added is approximately 1/2 to 1/3 that of ordinary calcium aluminate cement castables. Castables with a CaO content generally between 1.0% and 2.5% are called low-cement castables, while those with a CaO content less than 1.0% are termed ultra-low-cement castables.

 

 Compared with ordinary refractory castables, low-cement and ultra-low-cement castables differ in that their matrix uses ultrafine powders (particle size less than 1μm) with chemical compositions identical or similar to the main material of the castable to replace part or most of the calcium aluminate cement. Meanwhile, trace amounts of dispersants (water reducers) and a certain amount of delayed-action accelerators are added during preparation.

 

 Due to the replacement of calcium aluminate cement with ultrafine powders, low-cement and ultra-low-cement castables have the following advantages:

 

 (1) The lower CaO content in the castables reduces the formation of low-eutectic phases, thereby improving refractoriness, high-temperature strength, and slag resistance.

 

 (2) The water requirement of the castables is only 1/2 to 1/3 that of ordinary refractory castables, resulting in low porosity and high bulk density.

 

 (3) After molding and curing, fewer cement hydrates are generated. During heating and baking, there is no problem of significant mid-temperature strength degradation caused by the destruction of a large number of hydration bonds. Instead, the material gradually sinters with increasing heat treatment temperature, and the strength gradually improves.

 

The Mechanism of Setting and Hardening of Low-Cement and Ultra-Low-Cement Castables

 

 When compared with ordinary calcium aluminate cement castables, ordinary refractory castables mainly rely on the hydration of calcium aluminate minerals to generate CAH10, C₂AH6, C3AH8, and aluminum oxide gel for bonding, i.e., hydration bonding. In low-cement castables, however, hydration bonding and agglomeration bonding coexist; ultra-low-cement castables primarily rely on agglomeration bonding.

 

 The principle of agglomeration bonding is as follows: By adding electrolytes that slowly dissociate ions with charges opposite to those on the surface of ultrafine powder particles, the particles adsorb counterions dissolved from the electrolyte, reducing the zeta potential. When the adsorption reaches the "isoelectric point," agglomeration occurs, and the particles are bonded together via van der Waals forces. For example, in aluminum-silicon-based castables with SiO₂ ultrafine powder, the setting and hardening process is as follows: When the SiO₂ ultrafine powder is mixed with water, due to its high activity, it reacts with water to form colloidal particles. The surface of these colloidal particles carries a negative charge due to the dissociation of Si-OH groups into Si-O⁻ and H⁺. The negatively charged colloidal particles adsorb Al³⁺ and Ca²⁺ ions slowly released during the hydrolysis of calcium aluminate, reducing the zeta potential on the colloidal particle surface. When the adsorption reaches the "isoelectric point" (i.e., the colloidal particles are uncharged), agglomeration occurs, resulting in bonding.

 

 The setting and hardening mechanism of ultra-low-cement refractory castables is dominated by agglomeration bonding, with cement acting as a delayed accelerator. For instance, when SiO₂ ultrafine powder is added, it forms colloidal particles upon contact with water and adsorbs Al³⁺ and Ca²⁺ ions slowly released during the hydration of calcium aluminate, reducing the zeta potential. Setting and hardening occur when the isoelectric point is reached. Additionally, silanol groups form on the surface of active SiO₂, which dehydrate and form a siloxane network structure during drying. Simultaneously, the adsorption of Al³⁺, Ca²⁺, and Na⁺ ions from electrolytes also contributes to setting and hardening.

 

The Formulation Principles of Low-Cement Refractory Castables

 

 The formulation principles of low-cement refractory castables involve the rational selection of particle gradation, ultrafine powders, and types and dosages of admixtures. Refractory aggregates and powders are made from well-burned clay clinkers and high-alumina bauxite clinkers. The maximum particle size of refractory aggregates is determined by the thickness of the engineering lining, generally 10mm. The particle gradation is as follows: 10~5mm, 30%~40%; 5~3mm, 20%~30%; 3~0.15mm, 30%~40%. Generally, when formulating low-cement refractory castables, unified materials are rarely used; instead, three or four grades of gradation are employed to achieve the maximum packing density. The dosage of refractory aggregates is 68%~72%.

 

 Refractory powders typically use second-grade, first-grade, or special-grade high-alumina bauxite clinkers as raw materials. After grinding, iron removal treatment should be carried out, and the fineness of <0.09mm or <0.044mm should be ≥90%. They can be used alone or in proportion during formulation. Sometimes, high-grade materials such as alumina powder, white corundum powder, or brown corundum powder of the same fineness are added to improve the matrix performance of low-cement refractory castables. The dosage of refractory powders is 18%~25%, among which high-grade materials account for 5%~10% if added.

 

 There are many types of refractory ultrafine powders. Activated SiO₂ powder (i.e., silica fume) is commonly used at home and abroad, along with α-Al₂O₃ powder, Cr₂O₃ powder, SiC powder, etc. Their dosage is 2%~12%. The total dosage of refractory powders and ultrafine powders is 28%~32%. It should be noted that the dosage of ultrafine powders varies with different types of low-cement refractory castables, and corresponding optimal dosages need to be determined through experiments. The empirical optimal dosage is 4%~10%.

 

 In low-cement refractory castables, the main admixtures used are high-efficiency water reducers and dispersants, including NNO, MF, NF, JN, SM, humic acid, citric acid, tartaric acid, and their salts, sodium tripolyphosphate, sodium hexametaphosphate, boric acid, etc., with a general dosage of 0.03%~1.0%. When selecting admixtures, compatibility with ultrafine powders should be considered, as well as material sources, ease of use, and cost. Generally, organic admixtures have better water-reducing and dispersing effects than inorganic ones. Additionally, expanders such as kyanite and sillimanite are added to make low-cement refractory castables slightly expand at high temperatures.

 

 With a good understanding of these basic formulation principles, various types of low-cement refractory castables can be prepared. For example, a castable formulated with 70% first-grade bauxite clinker aggregate (8~0mm), 20% bauxite clinker powder of the same grade, 5% CA-50 cement (grade 625), 5% silica fume, 0.2% sodium tripolyphosphate, and 6.5% water has a dry compressive strength of 20MPa, a compressive strength of 72MPa after firing at 1450°C, and a linear shrinkage of 0.01%. In the above mix ratio, 0.03% tartaric acid and 0.05% borax or 0.3% sodium humate can also be used to prepare good low-cement refractory castables. The water dosage is generally not more than 7%, and less is better.

 

Composition of Low-Cement and Ultra-Low-Cement Castables

 

 The composition of low-cement and ultra-low-cement castables includes: refractory aggregates, refractory powders, an appropriate or small amount of calcium aluminate cement (delayed hardener), and trace dispersants (high-efficiency peptizing agents). The particle size composition requires multi-level batching, divided into 5~3mm, 3~1mm, 1~0.2mm, 0.2~0.074mm, 0.074~0.044mm, and micron levels. The proportion of different particle sizes can be calculated according to the Furness batching curve.

 

Applications of Low-Cement and Ultra-Low-Cement Castables

 

 The service temperature of low-cement and ultra-low-cement castables is higher than that of ordinary refractory castables with the same material. Clay-based and high-alumina low-cement castables can be used for the linings of various heat treatment rotary kilns such as reheating furnaces and soaking furnaces. Mullite-based low-cement castables are suitable for linings of high-temperature burners, wrapping linings for water-cooled pipes in reheating furnaces, and other applications. Corundum and chrome-containing corundum low-cement refractory castables can be used as linings for certain components in molten steel secondary refining devices, such as integral lance linings for injection metallurgy, immersion tube linings for RH or DH vacuum degassing units, as well as linings for power frequency induction furnaces and high-temperature wear-resistant linings for petrochemical fluid catalytic cracking reactors. Al₂O₃-SiC-C low-cement castables can serve as linings for high-alumina iron troughs, iron notch troughs in cupolas, and integral powder injection lances for hot metal pretreatment. MgO-Al₂O₃ or Al₂O₃-MgO-Al₂O₃ low-cement castables are suitable for ladle linings, steel tapping troughs, and other similar linings.

 

 

 

Low-cement SiC-based refractory castable

 

 The low-cement SiC-based refractory castable is characterized by low linear expansion coefficient, high thermal conductivity, high strength, and excellent wear resistance. It has been applied in thermal equipment such as power generation boilers, nonferrous metallurgical furnaces, and incinerators, achieving good performance.

 

 This castable uses silicon carbide (SiC) with a purity of over 97% as refractory aggregate and powder, adds SiO₂ ultrafine powder and metallic silicon as an antioxidant, employs CA-70 cement as a binder, and incorporates polyphosphate water-reducing agents. Its main properties are as follows:

 

SiC content: 85%

 

After drying at 110°C: Bulk density 2.5 g/cm³, compressive strength 45 MPa, flexural strength 9 MPa

 

After firing at 1000°C: Linear change -0.2%, compressive strength 107 MPa, flexural strength 24 MPa

 

After firing at 1450°C: Linear change +0.3%, compressive strength 130 MPa, flexural strength 54 MPa

 

Thermal conductivity at 400°C: 12.2 W/(m·K)