How Much High-Temperature Pitch Powder Maximizes Iron Trough Castable Performance?

Jan 27, 2026

Leave a message

 

Optimal Addition Level of High-Temperature Pitch Powder in Iron Trough Castables

 

Alumina–silicon carbide–carbon castables are widely used in the iron casthouse of modern blast furnaces. The main causes of damage to iron trough castables are as follows: reactions between the castables and molten iron and slag, which form eutectic mixtures and lead to failure; physical scouring by the flowing molten iron; and oxidative loosening of the castables during service, resulting in degradation and failure.

 

With the advancement of smelting technology, blast furnaces are becoming increasingly large in scale and higher in production capacity, which imposes more stringent requirements on refractory materials. Refractories are required not only to possess sufficient strength to ensure good castability, but also to exhibit excellent corrosion resistance to withstand the erosion and scouring of molten iron and slag. Therefore, the selection of a suitable carbon source is particularly critical.

 

Spherical pitch has a low fixed carbon content of only 60–70% and tends to form a porous structure in samples after firing, making it susceptible to oxidation. Flake graphite has a significant adverse effect on the flowability of castables: its flaky morphology requires a high water addition, which inevitably increases porosity and reduces the density of the material. In contrast, high-temperature pitch powder (fixed carbon ≥80%) and CarboresP (fixed carbon ≥80%) are amorphous carbon sources with high fixed carbon content, characterized by fine particle size, regular particle shape, and high reactivity. Moreover, their incorporation imparts excellent thermal shock resistance, low high-temperature creep, and poor wettability with molten iron and slag.

 

These two carbon sources are commonly used in carbon composite refractory products such as magnesia–carbon bricks and slide gate plates. Their addition can reduce the erosion and penetration of molten steel into refractories, thereby extending the service life of refractory materials and achieving favorable application results.

 

Therefore, incorporating a composite carbon source composed of high-temperature pitch powder and CarboresP into Al₂O₃–SiC–C iron trough castables is expected to improve their service performance. This paper investigates the effects of the addition amount of the composite carbon source on the room-temperature physical properties, high-temperature modulus of rupture, and oxidation resistance of Al₂O₃–SiC–C castables, and applies the research findings to industrial trials.

 

01. Experiments

 

1.1 Raw Materials

 

The main raw materials used in this study are as follows: brown fused alumina, white fused alumina, 97% silicon carbide, silica fume (particle size distribution: D50 < 1.7 μm), high-temperature pitch powder, CarboresP, high-alumina cement, metallic silicon powder (w(Si) = 98%), and activated alumina micropowder (particle size distribution: D50 < 1.8 μm). The chemical compositions of the main raw materials are presented in Table 1.

 

1

 

1.2 Sample Preparation

 

The experiment was conducted in two steps. First, the optimal addition amount of high-temperature pitch powder in brown fused alumina–based iron trough castables for this system was determined, and the corresponding formulation is shown in Table 2. Then, based on this formulation, the optimal addition amount of CarboresP was determined, with the corresponding formulation shown in Table 3.

 

2

 

3

 

The raw materials were batched according to the formulations shown in Tables 2 and 3. The prepared materials were first dry-mixed for 60 s, followed by the addition of a fixed amount of water based on construction operability requirements (4.5% water for the formulations in Table 2 and 4.8% for those in Table 3), and then wet-mixed for 120 s. The uniformly mixed slurry was cast into molds and formed by vibration on a vibrating table to prepare bar specimens with dimensions of 40 mm × 40 mm × 160 mm.

 

The specimens were cured in molds at room temperature for 18 h, then demolded and dried in a constant-temperature oven at 110 °C for 16 h. Subsequently, the specimens were fired in an air atmosphere at 1000 °C and 1500 °C, respectively, with a holding time of 3 h at each temperature, and finally cooled naturally to room temperature inside the furnace.

 

1.3 Performance Testing

 

The vibrating fluidity of the castables (25 vibrations within 30 s) was measured using a TZ-345 mortar fluidity tester. The bulk density and apparent porosity of the specimens after drying and firing were tested in accordance with GB/T 5072-2008 and GB/T 2997-2000, respectively. The compressive strength of the specimens after drying and firing was determined in accordance with YB/T 5201-1993.

 

The high-temperature modulus of rupture was tested in accordance with GB/T 3002-1982, with heat preservation at 1450 °C for 1 h in an air atmosphere. The dimensional changes of the specimens before and after firing were measured in accordance with GB/T 3001-2007 to calculate the linear change after firing. The microstructure of the fracture surfaces of the specimens after high-temperature rupture was observed using an EVO18 scanning electron microscope (SEM) manufactured by Carl Zeiss (Germany).

 

02. Analysis and Discussion of Experimental Results

 

2.1 Effect of High-Temperature Pitch Powder Addition on Room-Temperature Physical Properties of Castables

 

2.1.1 Effect of High-Temperature Pitch Powder Addition on the Fluidity of Castables

 

Under the same water addition conditions, the variation in fluidity with increasing high-temperature pitch powder content is shown in Figure 1. As can be seen from Figure 1, the fluidity of the castables first increases and then decreases with increasing addition of high-temperature pitch powder; deterioration in fluidity occurs when the external addition exceeds 2%.

 

This behavior can be attributed to the good dispersibility and fine particle size of the high-temperature pitch powder. A small addition amount can fill pores within the castables, reduce water demand, and thus improve fluidity. However, excessive addition causes the powder to remain outside the pore structure, leading to a decline in fluidity.

 

4

 

2.1.2 Effect of High-Temperature Pitch Powder Addition on Bulk Density and Apparent Porosity of Castables

 

The variations in bulk density and apparent porosity of the samples treated at different temperatures with varying amounts of high-temperature pitch powder are shown in Figure 2.

 

As shown in Figure 2(a), the bulk density of the castables first increased and then decreased after treatment at 110 °C for 16 h, 1000 °C for 3 h, and 1500 °C for 3 h, reaching a maximum at an external addition of 2% high-temperature pitch powder. Figure 2(b) shows that the apparent porosity of the samples first decreased and then increased under low, medium, and high-temperature treatments, with a minimum value observed at an external addition of 2% high-temperature pitch powder.

 

The reasons for these trends are as follows. First, a small increase in the addition of high-temperature pitch powder fills pores, densifies the structure, and promotes sintering, resulting in higher bulk density. Second, the bulk density of high-temperature pitch powder is approximately 1.35 g/cm³; replacing higher-density white fused alumina powder with pitch powder reduces the overall bulk density of the castables. Finally, excessive addition of high-temperature pitch powder decreases the fluidity of the castables and reduces structural compactness, leading to a decrease in bulk density and an increase in apparent porosity.

 

5

 

2.1.3 Effect of High-Temperature Pitch Powder Addition on Room-Temperature Compressive Strength of Castables

 

The variation in room-temperature compressive strength of the samples after heat treatment at different temperatures with varying amounts of high-temperature pitch powder is shown in Figure 3.

 

As shown in Figure 3, with increasing high-temperature pitch powder content, the room-temperature compressive strength of the samples dried at 110 °C shows little change. In contrast, the compressive strength of the samples fired at 1000 °C and 1500 °C first increases and then decreases, reaching a maximum at an addition of 2% high-temperature pitch powder.

 

Many factors influence the strength of the samples, including compactness, phase composition, and microstructure. The variation in strength after drying and firing can be attributed to the properties of high-temperature pitch powder: as an amorphous carbon source, an appropriate addition amount is well dispersed in the castables, fills the pores, and promotes densification and sintering of the material.

 

6

 

2.1.4 Effect of High-Temperature Pitch Powder Addition on High-Temperature Modulus of Rupture of Castables

 

The effect of high-temperature pitch powder addition on the high-temperature modulus of rupture of the castables is shown in Figure 4. As shown in Figure 4, the high-temperature modulus of rupture increases with increasing high-temperature pitch powder content, while only a slight increase is observed when the addition exceeds 2%.

 

This behavior can be attributed to the densification of the green body and the formation of a well-developed mullite crystalline phase at high temperatures. The presence of mullite significantly enhances the high-temperature modulus of rupture of the castables.

 

7

 

The above results indicate that adding different amounts of high-temperature pitch powder to iron trough castables can improve their fluidity, bulk density, and strength. The castables exhibit optimal overall performance when 2% high-temperature pitch powder is added. Therefore, the optimal mass fraction of high-temperature pitch powder in the iron trough castables for this experiment is 2%.

 

2.2 Determination of CarboresP Addition Amount

 

2.2.1 Effect of CarboresP Addition on Linear Change Rate of Castables after Different Temperature Treatments

 

The variation in linear change rate of the samples fired at 1000 °C and 1500 °C with different CarboresP additions is shown in Figure 5. All samples exhibit positive linear change after firing at 1000 °C for 3 h and 1500 °C for 3 h, indicating expansion.

 

For samples fired at 1000 °C, the linear expansion rate gradually increases with increasing CarboresP content. This is because carbon (C) and silicon (Si) react in situ at 800–1200 °C to form primary silicon carbide (SiC) crystals, which causes expansion. As CarboresP content increases, more SiC is generated, leading to greater expansion.

 

For samples fired at 1500 °C, the linear expansion rate first increases and then decreases, reaching a maximum at 1% CarboresP addition. The initial increase in expansion (0–1% CarboresP) is due not only to SiC formation but also to the mullitization reaction between Al₂O₃ and SiO₂, which also causes volume expansion. The subsequent decrease in expansion at 1.5% CarboresP may be related to a reduction in structural compactness.

 

8

 

2.2.2 Effect of CarboresP Addition on Room-Temperature Compressive Strength of Castables

 

The variation in room-temperature compressive strength of the samples with different CarboresP additions after various temperature treatments is shown in Figure 6. For samples dried at 110 °C, the compressive strength shows little change with increasing CarboresP content. In contrast, the compressive strength of the samples fired at 1000 °C and 1500 °C first increases and then decreases, reaching a maximum at a CarboresP addition of 1%.

 

The strength of the castables after drying mainly derives from the bonding between cement and composite micropowders in the matrix. Increasing CarboresP affects the fluidity of the castables, which in turn influences their bulk density. After firing, the strength is primarily controlled by the content of ceramic phases and low-melting phases formed at high temperatures. CarboresP contains low-melting substances, and excessive addition leads to the formation of a large amount of low-melting phases in the samples. Additionally, oxidation of residual carbon at high temperatures can loosen the sample structure, further reducing strength.

 

A comparison of compressive strength for different CarboresP contents indicates that an appropriate addition of CarboresP ensures good dispersion in the castables, fills pores, and promotes sintering of the green body. The castables achieve optimal strength after all temperature treatments when the CarboresP addition is 1%.

 

9

 

2.2.3 Effect of CarboresP Addition on the Oxidation Resistance of Samples

 

The morphologies of the sample cross-sections (40 mm × 40 mm) after heat treatment at 1000 °C for 3 h and 1500 °C for 3 h are shown in Figure 7. As shown in Figure 7, the degree of oxidation at 1500 °C is lower than that at 1000 °C, primarily because a denser oxide film forms on the sample surface at 1500 °C, which reduces oxidation. The thickness of the decarburized layer gradually decreases with increasing CarboresP content, improving the oxidation resistance of the samples. The samples show comparable oxidation resistance when the CarboresP content is 1% or 1.5%.

 

This behavior is mainly due to the gradual carbonization of CarboresP at high temperatures, with ceramic volatiles penetrating the material's voids and blocking pores. Therefore, an appropriate addition of CarboresP enhances the density and oxidation resistance of iron trough castables. However, excessive CarboresP addition reduces the fluidity of the castables and increases apparent porosity, leading to a lower density, a looser structure, and a corresponding decrease in oxidation resistance.

 

10

 

2.2.4 Effect of CarboresP Addition on High-Temperature Modulus of Rupture of Castables

 

The effect of CarboresP addition on the high-temperature modulus of rupture of the castables is shown in Figure 8. As shown in Figure 8, the high-temperature modulus of rupture increases with increasing CarboresP content, with only a slight further increase when the addition exceeds 1%.

 

Figure 9 presents micrographs of the fracture surface of the sample without CarboresP after high-temperature rupture, while Figure 10 shows the micrographs of the fracture surface of the sample with 1% CarboresP. A denser structure is clearly observed in the sample containing 1% CarboresP.

 

An appropriate addition of CarboresP fills the pores and promotes sintering. Excessive CarboresP, however, reduces fluidity, decreases the density of the castables, and may even damage the structure. Oxidation of carbon at high temperatures can further loosen the structure. Therefore, excessive CarboresP significantly reduces the high-temperature strength of the castables. The results indicate that adding 1% CarboresP forms a denser mullite crystalline phase and improves high-temperature rupture resistance.

 

11

 

12

 

13

 

In the Al₂O₃-SiC-C iron trough system, optimal comprehensive performance is achieved with 2% high-temperature pitch powder combined with 1% CarboresP as the optimal dosage.

 

03 Industrial Test and Application

 

Based on the research results, a brown fused alumina-based Al₂O₃-SiC-C castable prepared with a composite carbon source of 2% high-temperature pitch powder and 1% CarboresP was subjected to an industrial test at a steel plant in Tangshan. The blast furnace has a capacity of 1080 m³, with a 15 m long main trough to the small pit and an 11 m long slag trough, consuming 65 t of ramming mix (45 t for the main trough). The castable remained in service for 83 days until the next dismantling, with a total iron output of 165,000 t. In terms of refractory consumption per ton of iron, the castable demonstrated favorable application performance.

 

04 Conclusions

 

(1)With increasing high-temperature pitch powder addition, the room-temperature physical properties of the Al₂O₃-SiC-C castable show little change; the compressive strength first increases and then decreases, while the high-temperature modulus of rupture gradually increases. The castable exhibits the best overall performance when 2% high-temperature pitch powder is added.

 

(2)On the basis of 2% high-temperature pitch powder, the additional incorporation of 1% CarboresP further improves the performance of the iron trough castable and enhances its oxidation resistance. Excessive CarboresP addition, however, increases water demand and porosity and reduces strength.

 

(3)The brown fused alumina-based Al₂O₃-SiC-C castable prepared with a composite carbon source of 2% high-temperature pitch powder and 1% CarboresP (both by mass fraction) features good workability, easy curing, and excellent performance. Applied in the iron casthouse of a large blast furnace, it achieved a one-time iron throughput of 165,000 t, demonstrating promising industrial application results.