Research on Spalling & Wear-Resistant Castables for Cement Rotary Kiln Chute Openings
The refractory materials used at the chute opening of cement rotary kilns are among the most vulnerable components in cement plant equipment. Refractory damage arises from various causes: abrasion by clinker, chemical reactions with the coating, and deformation of the steel shell due to kiln rotation, among others. Additionally, cement plants play a pivotal role in the circular economy, where the recycling of waste as raw materials is widely practiced. As a result, damage caused by foreign components in waste raw materials has been increasing. Against this backdrop, refractory materials must possess excellent corrosion and wear resistance. This is why high-strength castables, including SiC-containing high-strength castables (hereinafter referred to as SiC-containing castables), which offer high durability for coatings and other applications, are commonly used.
During regular maintenance at cement plants, refractory construction at the chute opening is usually scheduled as the final process and must be completed within a limited timeframe before kiln ignition. Since construction occurs while the kiln is rotating, strict control of the construction duration is essential. Furthermore, the refractory materials at the chute opening are located close to the burner during ignition, requiring sufficient spalling resistance. At the same time, the durability of the refractory materials is crucial for stable operation during kiln running.
This paper presents the development of wear-resistant castables containing 10%–15% SiC, which are used in relatively small quantities in Japan, as well as the results of their application at the chute opening of cement rotary kilns. It also discusses their durability performance after approximately one year of service at the chute openings and air-quenched coolers.
01. Development of Materials
1. Determination of Adhesion with SiC Addition
1.1 Test Method
Clinker powder was placed on four types of high-strength castables with different SiC addition levels, followed by firing at 1450 ℃ to evaluate adhesion properties. The high-strength castables were molded into test specimens measuring 114 mm × 114 mm × 25 mm and then dried at 110 ℃. The clinker was collected from the kiln and crushed to a particle size of 0.15 mm. Three grams of the crushed clinker, formed into pellets of φ20 mm × 2 mm, were placed on each test specimen.
1.2 Test Results
Figure 1 shows photographs of the specimens after firing.

Silicon carbide (SiC) was added to the high-strength castable, which caused the clinker deposits to melt more easily; in addition, blistering was observed. It is speculated that this blistering is attributable to the reaction between SiC and the clinker deposits (SiC + 2O₂ → SiO₂ + CO₂), which generates CO or CO₂ gas, and the generated gas forms bubbles within the molten material. Furthermore, for test samples with an SiC addition level greater than 15%, the impact generated during cutting caused partially molten clinker deposits to detach and fall off. Based on these observations, it is inferred that the addition of SiC improves the spalling resistance of the castable.
Based on the above results and considering the actual application of SiC-containing castables with an SiC addition level of 10%–15% in overseas cement plants, a high-strength castable with an SiC addition level of 10%–15% was developed. Taking into account factors such as raw material costs, the castable with an SiC content of 12% developed in this project is described in detail below.
02 Physical Property Tests
Table 1 lists the typical values of the general physical properties of the SiC-containing castable and the conventional high-strength castable.

2.1 Wear Resistance Test
(1) Test Method
A wear loss test (in accordance with ASTM C704) was conducted to compare the wear resistance of the materials.
Samples of the high-strength castable and the SiC-containing castable were dried at 110 °C for 24 hours. The dried samples were then fired at 600 °C, 900 °C, 1000 °C, 1100 °C, 1200 °C, and 1300 °C for 5 hours at each temperature.
(2) Test Results
The results of the wear resistance tests under various temperature conditions are presented in Table 1, and photographs of the samples after the wear tests are shown in Figure 2. The wear resistance of the SiC-containing castable was essentially the same as that of the high-strength castable.

2.2 High-Temperature Linear Expansion Test
(1) Test Method
The high-temperature linear expansion coefficients of the high-strength castable and the SiC-containing castable were determined in accordance with JIS R2207-1.
(2) Test Results
The high-temperature linear expansion coefficients are presented in Table 1. The coefficient of the SiC-containing castable was 6.0 × 10⁻⁶/°C, whereas that of the high-strength castable was 7.0 × 10⁻⁶/°C, indicating that the SiC-containing castable has a lower high-temperature linear expansion coefficient.
2.3 Spalling Resistance Test
(1) Test Method
Samples of the high-strength castable and the SiC-containing castable were prepared and formed into specimens with dimensions of Φ80 mm × 80 mm. The specimens were then cured at 20 °C for 24 hours, after which they were placed in a furnace maintained at each test temperature to evaluate spalling behavior.
(2) Test Results
The results of the spalling resistance tests are listed in Table 1. The spalling resistance of the SiC-containing castable was equivalent to that of the high-strength castable.
2.4 Thermal Shock Resistance Test
(1) Test Method
The high-strength castable and the SiC-containing castable were formed into specimens with dimensions of Φ160 mm × 40 mm × 40 mm and cured at room temperature for 24 hours, followed by drying at 110 °C for an additional 24 hours. The dried specimens were cut at the center to produce two sub-specimens, each with dimensions of Φ80 mm × 40 mm × 40 mm. A specified amount of clinker powder was placed on the Φ40 mm × 40 mm surface of one sub-specimen, and the other sub-specimen was placed on top, with its Φ40 mm × 40 mm surface in contact. The assembled specimens were then fired at 1450 °C for 5 hours. After firing, a three-point bending test was conducted for evaluation, with the fracture load used as an indicator of adhesion strength.
(2) Test Results
The adhesion strength, specimen appearance, and fracture surfaces are shown in Figure 3.

As shown in Figure 3, the SiC-containing castable exhibits lower adhesion strength but higher thermal shock resistance compared with the high-strength castable without SiC addition. Observation of the fracture surfaces after the test revealed that the SiC-containing castable fractured at the blistered areas of the clinker powder, whereas the high-strength castable without SiC addition fractured in the matrix.
2.5 Workability Test for Chute Opening Application
(1) Test Method
The SiC-containing castable, as well as SiC-containing castables with the addition of a% and 2a% of additives, were each mixed separately. A flow cone with a 100 mm insert depth was placed on the inner base of the test setup, and a fixed vibration (2800 r/min for 10 s) was applied. The spread of the material was measured to determine changes in fluidity over time. Fluidity measurements were taken immediately after mixing, and at 5, 10, 15, 20, 25, 30, 60, and 120 minutes post-mixing.
(2) Test Results
The change in fluidity over time is shown in Figure 4. It can be seen that the SiC-containing castable maintained stable fluidity for more than 2 hours without any additives. Furthermore, the setting time can be easily controlled by adjusting the dosage of the additive.
2.6 Study on the Addition of Metal Fibers to SiC-Containing Castables
(1) Determination of Physical Properties of SiC-Containing Castables with Metal Fibers Added
Metal fibers were incorporated into the refractory material for kiln chute openings, and the corresponding physical properties were measured.
① Spalling Resistance Test
② Test Method
SiC-containing castables with 1% and 2% metal fibers added were prepared as test specimens. The test method was the same as described above.
③ Test Results
The results of the spalling resistance tests are presented in Table 2. The addition of metal fibers to the SiC-containing castables was found to result in a tendency toward reduced spalling resistance.

(2) Wear Resistance Test
① Test Method
SiC-containing castables with 1% and 2% metal fibers added were prepared as test specimens. The test method was the same as described above.
② Test Results
The addition of metal fibers to the SiC-containing castables was found to cause a slight reduction in wear resistance.
Based on the above results, no improvement in spalling resistance or wear resistance was observed with the addition of metal fibers to the SiC-containing castables.
03 Industrial Kiln Service Performance
3.1 Service Performance at the Chute Opening
Figure 5 shows the service results at the chute opening after approximately one year of operation following construction, during which the refractory at this location was replaced simultaneously with the kiln coating. No maintenance was performed, and production continued for six months; minor chipping was observed after one year of operation, with no occurrence of spalling or other damage.

3.2 Service Performance in the Air-Quenched Cooler
Figure 6 presents the service results after approximately 1.5 years of operation following construction.
The matrix remained intact with excellent durability, and the material continues to be in service to date.

The matrix remains intact with excellent durability and is still in continuous service to date.
04 Conclusions
This paper has presented the development, industrial kiln application, and actual service performance of the SiC-containing castable for cement plants. The research findings indicate that this castable can effectively control clinker adhesion at the kiln chute opening, enabling continuous production for six months without any repairs, and its one-year service life has been verified. In addition, it has achieved a service life of over 1.5 years in the air-quenched cooler. From construction to actual operation, this SiC-containing castable has contributed to ensuring stable production in cement plants.