Continuing from the previous post...
2.1.4 Cold Modulus of Rupture and Hydration Resistance
Figure 5 shows the cold modulus of rupture and hydration weight gain rate of MgO-CaO specimens doped with Y₂O₃ and ZrO₂, respectively. The cold modulus of rupture of MgO-CaO specimens with single Y₂O₃ doping increases gradually. At low Y₂O₃ addition, the densification of specimens is improved and the bonding between main crystalline phases is strengthened, thus increasing the cold modulus of rupture of specimens. When the Y₂O₃ addition is high, the apparent porosity of specimens rises significantly, which degrades the mechanical properties of the material. Nevertheless, Y₂O₃ distributed at grain boundaries tightly bonds with the main crystalline phases and acts as a bridging phase, which is beneficial to the improvement of mechanical properties.
With the increase of Y₂O₃ content, the hydration resistance of the material rises first and then declines. When the Y₂O₃ addition reaches 10 mol%, the formation of yttrium-rich banded zones on the surface of CaO grains hinders the hydration reaction of free CaO, which contributes to better hydration resistance. However, the marked increase in apparent porosity enlarges the contact area between CaO grains and water vapor, resulting in deteriorated hydration resistance of the material.

Figure 5 Cold modulus of rupture and hydration weight gain rate of MgO-CaO specimens singly doped with Y₂O₃ and ZrO₂
The cold modulus of rupture of MgO-CaO specimens singly doped with ZrO₂ increases first and then decreases with the rise of ZrO₂ addition. At low ZrO₂ addition, the material achieves high sintered density and the CaO grain size is refined, which is conducive to improving the cold modulus of rupture. In contrast, when excessive ZrO₂ is added, the increase in apparent porosity leads to deterioration of the material's mechanical properties.
For MgO-CaO specimens incorporated with different ZrO₂ contents, the hydration weight gain rate decreases first and then increases. The minimum hydration weight gain rate of 5.37 wt% is obtained at ZrO₂ addition of 1 mol%. This is because a small amount of ZrO₂ added into MgO-CaO specimens produces a dense microstructure with a high degree of direct grain bonding. The bonding between CaO and MgO is enhanced, and the contact area between CaO and water vapor is reduced. The formed CaZrO₃ is resistant to hydration, which reduces the content of free CaO in the system. Part of the free CaO is encapsulated by MgO and CaZrO₃ particles, further improving the hydration resistance of the material.
2.2 Y₂O₃/ZrO₂ Co-doped MgO-CaO Refractories
2.2.1 Phase Composition
Figure 6(a) shows the XRD patterns of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens. When the molar ratio n(ZrO2):n(CaO) is 0.5:100 and 1:100, the formation amount of CaZrO₃ in specimens YZ0.5 and YZ1 is very low, and the diffraction peaks of CaZrO₃ are inconspicuous. When n(ZrO2):n(CaO) increases to 3:100, obvious CaZrO₃ diffraction peaks are observed in specimen YZ3. With further increasing ZrO₂ addition, the diffraction peak intensity of CaZrO₃ in specimen YZ6 gradually rises.
As shown in Figure 6(b), compared with specimen Z3, the main peak position of CaZrO₃ in specimen YZ3 shifts toward higher angles. According to Bragg's law, the crystal lattice and unit cell parameters of CaZrO₃ decrease. This is because Y³⁺ from Y₂O₃ substitutes for Ca²⁺ in CaZrO₃ in specimen YZ3, generating Ca²⁺ vacancies, as shown in Equation (6). The formation of point defects can induce lattice distortion, activate the crystal lattice and promote the sintering of materials.


Figure 6 XRD patterns of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens
2.2.2 Microstructure
Figure 7 shows FESEM images of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens with different compositions. Compared with specimen Y10, the pores in the co-doped specimens decrease first and then increase with the rising ZrO₂ addition, and the aggregated regions of bright white spherical particles gradually increase.
Figure 8 presents the FESEM image and EDS mapping results of specimen YZ1. According to the energy spectrum results, the dark grey regions in the micrograph correspond to periclase phase, the grey regions are lime phase, the bright white irregular blocky regions are Y₂O₃, and the stacked bright white spherical regions are CaZrO₃. Y₂O₃ and CaZrO₃ are distributed at grain boundaries.
Based on the point scanning results listed in Table 3, Y element exists in CaZrO₃ grains. Combined with the XRD analysis in Figure 6(b), it further demonstrates that part of Y₂O₃ is dissolved into CaZrO₃.
For Y₂O₃/ZrO₂ co-doped MgO-CaO refractories, a portion of Y₂O₃ dissolves into the crystal lattices of CaO and CaZrO₃, inducing lattice distortion, activating the crystal lattice and promoting material sintering. In contrast, another portion of Y₂O₃ resides in the intergranular regions of the main crystalline phases and hinders sintering.

Figure 7 FESEM images of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens

Figure 8 FESEM image and EDS mapping results of specimen YZ1
| Atomic fraction/% | |||||
|---|---|---|---|---|---|
| Sample ID | Mg | Ca | Y | Zr | O |
| Point 5 | 5.59 | 17.68 | 7.00 | 11.99 | 57.74 |
| Point 6 | 1.94 | 46.09 | 1.93 | - | 50.48 |
| Point 7 | 1.22 | 46.64 | 1.71 | - | 50.43 |
| Point 8 | 6.56 | 6.62 | 24.25 | 4.34 | 58.23 |
Table 3 EDS point scanning results of marked points in Figure 8
2.2.3 Sintering Properties
Figure 9 shows the linear shrinkage, apparent porosity and bulk density of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens with different compositions. The linear shrinkage and bulk density of the specimens increase first and then decrease with the gradual rise of ZrO₂ content, while the apparent porosity shows the opposite trend.
When a small amount of ZrO₂ is introduced, the volume expansion caused by the formed CaZrO₃ fills the pores inside the material and improves its densification. Meanwhile, the solid solution between CaZrO₃ and Y₂O₃ induces lattice distortion and promotes the sintering of the material. However, with further increasing ZrO₂ addition, the production of CaZrO₃ rises sharply, which brings about significant volume expansion and reduces the densification of specimens.

Figure 9 Linear shrinkage, apparent porosity and bulk density of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens
2.2.4 Cold Mechanical Properties and Hydration Resistance
Figure 10 shows the cold modulus of rupture and hydration weight gain rate of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens. With the increase in ZrO₂ addition, the cold modulus of rupture of specimens rises first and then falls, which is closely related to the variation of specimen densification. At the ZrO₂ addition of 1 mol%, the specimen achieves the maximum cold modulus of rupture of 89.98 MPa.
Compared with specimen Y10, the hydration weight gain rates of specimens YZ0.5 and YZ1 decrease slightly, while those of YZ3 and YZ6 increase further. When a small amount of ZrO₂ is introduced, the densification of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens improves, reducing the contact area between specimens and water vapor and enhancing the hydration resistance of the material.
In addition, MgO, Y₂O₃ and CaZrO₃ distribute around CaO grains, lowering the contact area between CaO grains and water vapor. The formation of CaZrO₃ stabilizes part of CaO and reduces the amount of free CaO, thereby improving the hydration resistance of the material. Meanwhile, part of Y₂O₃ forms a solid solution with CaO, which also exerts a positive effect on hydration resistance.
When excessive ZrO₂ is added, more CaZrO₃ is generated and the content of free CaO in the material is further reduced. Nevertheless, the volume expansion accompanied by substantial CaZrO₃ formation loosens the material microstructure and increases apparent porosity. This enlarges the contact area between the material and water vapor and consequently deteriorates the hydration resistance.

Figure 10 Cold modulus of rupture and hydration weight gain rate of Y₂O₃/ZrO₂ co-doped MgO-CaO specimens
3.Conclusions
When a small amount of Y₂O₃ is introduced into MgO-CaO refractories, Y³⁺ dissolves into the CaO crystal lattice and induces lattice distortion, which promotes sintering and improves the densification and hydration resistance of MgO-CaO refractories. At high Y₂O₃ addition, part of Y₂O₃ resides at grain boundaries and hinders sintering. The apparent porosity of the material increases, the contact area between water vapor and CaO expands, and the hydration resistance of the material decreases.
When a small amount of ZrO₂ is introduced into MgO-CaO refractories, the formed CaZrO₃ fills the grain boundaries and improves the material densification. The formation of CaZrO₃ stabilizes part of CaO and enhances the hydration resistance of the material. With excessive ZrO₂ addition, more CaZrO₃ is formed in the material. The resulting volume expansion reduces the densification and hydration resistance.
After the co-introduction of Y₂O₃ and ZrO₂ into MgO-CaO refractories, Y₂O₃ can dissolve into both CaO and CaZrO₃, generating Ca²⁺ vacancy defects, activating the crystal lattice and promoting sintering. When the ZrO₂ addition is 1 mol%, the specimen achieves relatively high densification and good hydration resistance. Further increasing ZrO₂ addition leads to a remarkable rise of CaZrO₃ formed at grain boundaries, accompanied by reduced densification and deteriorated hydration resistance.