Analysis of the reasons affecting the clogging of the water outlet of the intermediate packet and measures to solve the problem
In the continuous casting production process, the phenomenon of intermediate ladle nozzle clogging occurs frequently. This leads to a reduction in the casting speed or even interruption of the molten steel flow. Viscous slag materials inside the intermediate ladle nozzle can also cause flow deviation at the submerged nozzle, leading to slag entrapment, cracks, and other defects, which adversely affect normal production.
According to statistics, unplanned shutdowns caused by intermediate ladle nozzle clogging account for approximately 3.7% of total downtime. Experts at home and abroad have conducted extensive research on this issue. Drawing on their experience, the Continuous Casting Department has carried out long-term tracking and analysis.
In the continuous casting process, the role of the submerged nozzle is to control the flow rate of molten steel from the intermediate ladle to the mold and to direct the flow of steel within the mold. This function is crucial for stabilizing operations and ensuring steel quality.
When alumina adheres to the inner wall of the submerged nozzle, flow irregularities and steel level fluctuations in the mold can occur. This not only deteriorates the quality of the continuously cast billet but also severely affects the implementation of multi-heat continuous casting.
Process Overview
SPHC is one of the main varieties of low-carbon, low-silicon, aluminum-killed steel produced by our department. It follows the production process route of basic oxygen furnace (BOF) top and bottom blowing → LF refining furnace → continuous casting machine. However, during the casting process of this steel grade, nozzle clogging at the intermediate ladle frequently occurs, which affects normal production and results in unplanned casting interruptions.
Cause Analysis
There are two main phenomena associated with intermediate ladle nozzle blockage. One is caused by various factors leading to low-temperature flocculation of molten steel. In this case, pouring is interrupted due to blockage at the nozzle, where the outer ring contains dark gray material and the inner ring contains a small amount of white substances. The main components are Fe and FeO.
The other phenomenon involves the gradual buildup of deposits on the inner wall of the intermediate ladle nozzle. Over time, these deposits cause the inner diameter to narrow, eventually leading to complete blockage. The material causing the blockage is white and mainly composed of Al₂O₃.
01. Reasons for Clogging Material Mainly Composed of Fe and FeO
Insufficient Baking of the Intermediate Ladle Nozzle
Due to insufficient or unstable gas supply, irregular production in continuous casting often leads to frequent use of intermediate ladles. In some cases, the ladles are hastily used before meeting baking requirements. When molten steel is injected into a ladle with a nozzle area at relatively low temperature, cold steel may easily solidify, reducing the inner diameter of the nozzle or causing complete clogging.
Excessive Cooling of Molten Steel in the Intermediate Ladle During Casting
During the continuous casting process, if the molten steel temperature is too high or the casting speed is high, scrap steel is often added to the intermediate ladle to reduce temperature and prevent steel breakout. Since each steel grade has its own liquidus temperature, excessive cooling may cause the molten steel temperature to approach or reach the liquidus point, leading to partial solidification. Statistics show that when the superheat (ΔT) is less than 5 °C, the probability of flocculation is 100%. When ΔT is between 6–10 °C, the probability drops to 31%.
Molten Steel Temperature Not Meeting Standards
If the molten steel temperature itself is below standard, it can cause low-temperature dead zones and flow issues. This situation may occur under the following conditions:
(1)Inaccurate temperature measurement during converter tapping, leading to overly high molten steel temperatures and direct tapping without adequate adjustment.
(2)The ladle preheating temperature does not reach 800 °C before use, resulting in excessive temperature drop after receiving molten steel.
(3)A large piece of residual steel is left at the bottom of the ladle from the previous heat and not reported in time.
(4)During tapping, slag from the furnace mouth accidentally falls into the ladle.
02. Reasons Why the Main Component of the Clog Is Al₂O₃
Since SPHC steel is deoxidized using aluminum blocks and undergoes deep deoxidation, the primary deoxidation product is Al₂O₃. Observations revealed that flocculent material adhering to the inner wall of the submerged nozzle appears in two colors: dark yellow and blue. A similar material was also found on the surface of nearby nodular cold steel.
Electron microscopy analysis of the flocculent material from the nozzle showed that, although the appearance and color of the two samples were different, their chemical compositions were similar. Both were Al₂O₃-based oxides containing small amounts of CaO, SiO₂, and MnO. Morphologically, the blue bonding material appeared denser, while the yellow material was more porous. Chemical analysis of the bonding material on the surface of the nodular cold steel confirmed that its composition was identical to that of the material on the nozzle wall.
Cross-sectional analysis of the cold steel showed a large number of diffusely distributed inclusions. These inclusions can be divided into two main types:
MnS inclusions
Composite inclusions rich in Al₂O₃, CaO, SiO₂, MnO, and TiO₂.
The second type of inclusion typically appears irregular or nearly spherical, with a size of about 10 micrometers and fine particle distribution. Typical inclusion morphology shows Al₂O₃ particles at the core, surrounded by layers containing SiO₂, MnO, and CaO. This suggests that these inclusions likely originate from aluminum deoxidation products that failed to float out.
In more oxidized steel, Si and Mn deoxidation products - or secondary oxidation products - may form composite inclusions with Al₂O₃ as the core. These inclusions remain solid at continuous casting temperatures and gradually accumulate on the inner wall of the intermediate ladle nozzle. Calcium treatment in this case does not effectively convert Al₂O₃ into liquid calcium aluminate, and thus fails to prevent clogging, ultimately leading to nozzle blockage.
Measures Taken
01. Low-Temperature Flocculation Caused by Temperature
The following measures have been implemented:
(1)Regular inspection of gas baking pipelines for the intermediate ladle is conducted to prevent gas blockages or leaks. This ensures an adequate gas supply for baking. The principle of "small fire first, then medium, then large" is strictly followed to guarantee that the intermediate ladle reaches a temperature above 1,000 °C before use. Additionally, ladle lining buildup should not only meet production requirements but also maintain a safety margin for emergencies.
(2)Improve steel tapping temperature and composition control at the end of blowing to ensure that the molten steel entering the continuous caster has an appropriate temperature and meets compositional standards. If the molten steel temperature in the intermediate ladle is too low during casting, the casting start time should be delayed to raise the temperature and static pressure, allowing more time for inclusions to float out and increasing the success rate of casting.
(3)Prevent excessive cooling of molten steel in the intermediate ladle during pouring by requiring the ladle operator to measure the temperature of each heat at least three times. For carbon structural steel and low-alloy steel, the appropriate pouring temperature should be determined based on the chemical composition of each grade. The superheat of the molten steel should be maintained within the range of 10–20 °C, and ladle operators must strictly follow this standard.
02. Low-Temperature Flocculation Due to Al₂O₃
By adding a certain amount of calcium to the molten steel, the high-melting-point Al₂O₃ can combine with CaO to form low-melting-point calcium aluminates, which can more easily diffuse and float. To reduce the formation of manganese sulfide inclusions, calcium treatment of molten steel is commonly used. For calcium treatment to be effective, careful control of the calcium addition is essential. Improper calcium treatment not only fails to achieve the desired metallurgical effects but can also worsen the castability of the steel.
There are two main reasons why calcium treatment may lead to nozzle blockage:
Insufficient calcium addition – When the amount of calcium added is too low, Al₂O₃ is only partially converted into calcium aluminates such as CaO·6Al₂O₃, CaO·2Al₂O₃, CaO·Al₂O₃, or CaO·3Al₂O₃, rather than the fully modified 12CaO·7Al₂O₃. These partially converted phases have higher melting points and may cause accumulation and blockage.
Excessive calcium addition – When too much calcium is added, it reacts with sulfur in the steel to form CaS, which has a high melting point of around 2500 °C. As the calcium content increases, the calcium content in the inclusions also rises, leading to the formation of complex inclusions. Among them, compounds like CaO·6Al₂O₃ and CaO·2Al₂O₃ have melting points above 1700 °C and must be avoided in actual production.
To ensure proper calcium treatment:
Sufficient calcium must be added, with a recommended wire feeding rate of 1.5–2.5 meters per tonne of steel.
Adequate refining slag should be added to provide sufficient capacity to absorb inclusions.
Sulfur content in the steel must be controlled, and the coordination of sulfur and dissolved aluminum ([Alₛ]) in the steel should be optimized to reduce the likelihood of CaS formation. The sulfur content of incoming steel should be kept low.
Achieving the right balance of [Alₛ], S, and Ca ensures the effective modification of Al₂O₃ inclusions, reduces total oxygen content, and improves steel purity. After process optimization, the flocculation phenomenon at the continuous casting nozzle was largely resolved, and Al₂O₃ inclusions larger than 30 microns were effectively removed, leading to more stable continuous casting operations.
Calcium treatment of low-carbon, aluminum-deoxidized steel transforms Al₂O₃ inclusions into low-melting-point compounds, significantly improving castability and preventing adhesive nozzle clogging.
Conclusion
The main components of the clogging material-Fe and FeO-are primarily caused by insufficient baking of the intermediate ladle nozzle, excessive cooling of molten steel in the ladle, and substandard molten steel temperatures, all of which can result in low-temperature flocculation. These issues can be completely avoided through appropriate process improvements.
When the main component of the clogging material is Al₂O₃, it is due to the inability of aluminum deoxidation products (Al₂O₃) to float out in time, as well as improper calcium treatment.
To reduce the formation of CaS during calcium treatment of molten steel, it is essential to maintain a low sulfur content. The sulfur level in the incoming molten steel must be controlled. Effective coordination of dissolved aluminum ([Alₛ]), sulfur (S), and calcium (Ca) in the molten steel is required.